Welding materials SA-240 310s (P.no8) to SA-213 T11 (P.no4)

77 views
Skip to first unread message

Mohamed Elsayed

unread,
Aug 14, 2023, 7:26:21 AM8/14/23
to material...@googlegroups.com
Hello dears
I'm going to weld SA-240 310s (P.no8) to SA-213 T11 (P.no4), but I don't know what is the proper electrod or filler metal to weld this material, so help me please

Ahmed Osman

unread,
Aug 15, 2023, 10:57:16 PM8/15/23
to material...@googlegroups.com
* if PWHT is needed for 213 T11  ... cladding technique will be used ( 1st clad P4 with ERNiCr-3 then finalize PWHT ) (2nd weld with P8 with same electrode )
* If PWHT not needed for 213 T11 and
   - service temp. less 315c     -- use 309L
   - service temp. more 315C  -- go with ERNiCr-3

best regards
Ahmed Osman



On Monday, August 14, 2023 at 02:26:15 p.m. GMT+3, Mohamed Elsayed <m.say...@gmail.com> wrote:


Hello dears
I'm going to weld SA-240 310s (P.no8) to SA-213 T11 (P.no4), but I don't know what is the proper electrod or filler metal to weld this material, so help me please

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKujbmu2ZYjN8UsS-ko2PZu0YT1EUHFBV1JPHM8ZdNvRP65E_Q%40mail.gmail.com.

manish kulkarni

unread,
Aug 15, 2023, 10:57:16 PM8/15/23
to material...@googlegroups.com
Pl refer API RP 582 



On Monday, August 14, 2023, 3:26 PM, Mohamed Elsayed <m.say...@gmail.com> wrote:

Hello dears
I'm going to weld SA-240 310s (P.no8) to SA-213 T11 (P.no4), but I don't know what is the proper electrod or filler metal to weld this material, so help me please

--

Kannayeram Gnanapandithan

unread,
Aug 16, 2023, 12:22:47 AM8/16/23
to material...@googlegroups.com
what is the thickness. 
If Thickness is less than 13mm, Preheat T11 side and weld T11 + ASS with ER NiCr3
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349