Dear Sirs ,
We have a project with both shell and Reinforcement Pad materials SA516-70, 10 mm Thk ( P No.1 ) and the Nozzle is SA335-P22, 4” Sch 120 ,
11.1 mm ( P No.5A ) Thk.
We already have a qualified WPS & PQR with 8mm GTAW and tested about 10 years ago by other welding engineer, for P No,.5A to P No.1 without PWHT and it was satisfactorily passed and we
have used that WPS & PQR for the previous project 10 years ago and no
issues found without PWHT.
Now for the new project, we are going to use the same WPS and apply
Preheat ( 204 to 250 Deg C ) as per the WPS for 10mm Shell Thk by
multipass welding, refer to the below sketches.


So, i would like to confirm whether PWHT is mandatory as per UCS-56-4 ?
Can we avoid PWHT for this 10mm weld joint ?
Or Should we do buttering with ERNiCr-3 on P No.5A bevel and butt weld
with same filler for this dissimilar joint to avoid PWHT after making new
PQR with buttering?
Please confirm soon.
Thanks and Regards,
Saravanan Sornam,
ANSAN-Si,
S.Korea
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CALV1rk%2Biby3LDhuASFD6Sx3wD6mhOVKRXA8dsJCQcfO-yNsjhQ%40mail.gmail.com.
On 22 May 2025, at 2:26 PM, Raghuram Bathula <raghura...@gmail.com> wrote:
Why do you use P22 nozzles on CS?
On Thu, 22 May 2025, 16:24 PARAI Reaction Channel, <sarava...@gmail.com> wrote:
Dear Sirs ,
We have a project with both shell and Reinforcement Pad materials SA516-70, 10 mm Thk ( P No.1 ) and the Nozzle is SA335-P22, 4” Sch 120 ,
11.1 mm ( P No.5A ) Thk.
We already have a qualified WPS & PQR with 8mm GTAW and tested about 10 years ago by other welding engineer, for P No,.5A to P No.1 without PWHT and it was satisfactorily passed and we
have used that WPS & PQR for the previous project 10 years ago and no
issues found without PWHT.
Now for the new project, we are going to use the same WPS and apply
Preheat ( 204 to 250 Deg C ) as per the WPS for 10mm Shell Thk by
multipass welding, refer to the below sketches.
<image.png>
<image.png>
So, i would like to confirm whether PWHT is mandatory as per UCS-56-4 ?
Can we avoid PWHT for this 10mm weld joint ?
Or Should we do buttering with ERNiCr-3 on P No.5A bevel and butt weld
with same filler for this dissimilar joint to avoid PWHT after making new
PQR with buttering?
Please confirm soon.
Thanks and Regards,
Saravanan Sornam,
ANSAN-Si,
S.Korea
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CALV1rk%2Biby3LDhuASFD6Sx3wD6mhOVKRXA8dsJCQcfO-yNsjhQ%40mail.gmail.com.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CADxVub%3DgSEPtoFpp%2BtcafrEOrNOzUxFt_9E4TfiPwfyP21JHdg%40mail.gmail.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CADxVub%3DgSEPtoFpp%2BtcafrEOrNOzUxFt_9E4TfiPwfyP21JHdg%40mail.gmail.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CALV1rkJt_cnVR3wJkwRy%3DHUD9Qviu-HO7EmcYVbQQmmkV2v8iA%40mail.gmail.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAPOi40DG_DrGuXyUf71iiv7uhcJSQxtFTDnFfu%2B9TavjjOOrPg%40mail.gmail.com.