SS304/304L Tubes to CS Tubesheet Mock Weld -Cracks found

35 views
Skip to first unread message

PARAI Reaction Channel

unread,
Apr 15, 2026, 9:48:25 AMApr 15
to materials-welding@googlegroups com
Dear Sirs,

We have made 2 MockUp PQRs as per ASME Sec IX QW-193.

The Tube sizes are 19.05OD x2.11T and 15.88OD x2.11T, the
tubesheet plate is SA-516-70, 50T.

Amps used Max 145, Volts Max 13, welded with GTAW AWS Class ER309 with 1.6mm Filler , 2 passes.

We found minor cracks on the weld root and some on the surface too, but not for all the 10 tubes welded, but randomly found these cracks

When we did PT after welding on the surface, no cracks were found. But found after Macro etching at the test lab.

Can I switch the filler to ER309LMo for this MockUp weld ?

Are these cracks called Hot cracks ?

Please give me some advice.

With best regards,
Saravanan Sornam,
Ansan city,
S.Korea.


patni engineers

unread,
Apr 15, 2026, 10:37:12 AMApr 15
to material...@googlegroups.com
Check ER 347

Regards,

Chandrakant
B.E Mech.
ASNT Level II RT/UT/PT/MPT/CSWIP

GST -27AMOPP5962A1ZS
Patni Engineers. Mumbai. India
PED/2014/68/EU
welding shop AD2000/DIN EN ISO 3834
IBR Approved 

Factory Addreess- Pl Call 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CALV1rkLag0%3D-RPjKQhRB21ODF3eNenk1Ey71-xTpp5LFMvTj5w%40mail.gmail.com.

Vanchinath S.A.

unread,
Apr 15, 2026, 11:06:57 PM (14 days ago) Apr 15
to material...@googlegroups.com
Weld root with 80-90 amps. 
Vanchi

PARAI Reaction Channel

unread,
Apr 16, 2026, 1:32:13 AM (14 days ago) Apr 16
to materials-welding@googlegroups com
Dear Sir, 

Thank you for your advice for root welding parameters. 

Can i use ER309LMO  instead of ER309 ?

Please confirm. 

Thanks and regards, 
Saravanan Sornam, 
ANSAN,
S.KOREA 


Ahmed Osman

unread,
Apr 16, 2026, 5:22:00 AM (14 days ago) Apr 16
to materials-welding@googlegroups com
sure, 309LMO will be helpful as low carbon and MO are increasing delta ferrite for avoiding hot cracks
also reduce heat input for controlling dilution from CS sheet

Best Regards ,
Ahmed Osman