Dear master 

in our project we have a leak in fire water service and i want to know the repair procedure for the pipe 

ductile iron C151A21.51 

electrode rod using for andf procedure if possible 

Vishwas Keskar

unread,
Mar 25, 2021, 4:01:02 AM3/25/21
to material...@googlegroups.com
Use ENi CI electrodes with pre heating @200 Deg C 
Use Multipass welds 



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bd7269bd-a954-4c54-a816-2c3c45a84f3bn%40googlegroups.com.

luis carlos greggianin

unread,
Mar 25, 2021, 11:34:40 PM3/25/21
to material...@googlegroups.com
Use shot penning during the weld too

--

pgos...@rogers.com

unread,
Mar 26, 2021, 12:01:49 AM3/26/21
to material...@googlegroups.com

Hi Cast Irons are typically subjected to repair weld. The repair welding is normally done by Nickel based electrodes, 99% Ni or 55% Ni electrodes. This applies to any welding on new cast iron pipes also. It’s extremely difficult to meet ASME Sec-IX welding qualification criteria for Cast Iron Welding.

 

The links cited below would provide you good resources for Cast Iron Welding.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Engineering Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

 

Can You Weld Cast Iron? (A Complete Guide) - TWI (twi-global.com)

 

Sec. 8 Introduction (ductile.org)

From: luis carlos greggianin <luisca...@gmail.com>
Sent: March 25, 2021 5:53 PM
To: material...@googlegroups.com
Subject: Re: [MW:32090] ductile iron welding procedure

 

Use shot penning during the weld too

 

Em Qui, 25 de mar de 2021 00:13, QA/QC <adnan...@gmail.com> escreveu:

Dear master 

 

in our project we have a leak in fire water service and I want to know the repair procedure for the pipe 

 

ductile iron C151A21.51 

 

electrode rod using for and procedure if possible 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bd7269bd-a954-4c54-a816-2c3c45a84f3bn%40googlegroups.com.


Virus-free. www.avg.com
Reply all
Reply to author
Forward
0 new messages