peening as a temporary repair

593 views
Skip to first unread message

Adriaan Stoltz

unread,
Jun 24, 2014, 7:33:38 AM6/24/14
to material...@googlegroups.com

Good day valued members.

 

Has any of you gentlemen had any experience in temporary repairs on carbon steel pressure vessel by means of mechanical peening? A steam leak was discovered on a Low pressure Heater (300Kpa) at a nozzle to vessel shell weld interface. It seems to be a pinhole through the weld. Is mechanical peening of the defect area considered to be an acceptable means of closing up the leak temporarily until a proper weld repair can be carried out?  And if so, is this type of repair documented in any of the in service inspection and repair standards?

Your input is greatly appreciated.

 

 

Riaan Stoltz

RITC Inspection

083 6405909

021 556 4884

 

Ramesh Bapat

unread,
Jun 24, 2014, 10:13:18 PM6/24/14
to material...@googlegroups.com

I suggest against it in an existing vessel in steam service.  Peening may take care of a surface indication or stop up a pin hole leakage, but  one has no idea if the root cause may or may not be a lot bigger than what can visually be detected.  Steam is erosive. It will eat metal away fast.   Also if steam flashes, it can hammer, which will result in the possibility of high stress concentrations at points of stress risers in such as nozzle to shell welds (corner joints) which over time, can cause stress cracking.  I suggest you to take this vessel out of service, perform a UT examination at the location of the indication (Try to discover the path of failure), remove the defective weld to sound metal by grinding, PT examine the repair area, re-weld it, PT the cover pass, perform local PWHT if required by code, and re-hydro test it.  I would not risk the possibility of blowing a nozzle off the vessel wall for a quick fix of a leaky weld in steam service. Thanks

 

Ramesh Bapat

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

nishan...@yahoo.com

unread,
Jun 24, 2014, 11:48:13 PM6/24/14
to material...@googlegroups.com

Dear all,
Greetings from my side,

I too agree to the fact that Mr. Bapat has mentioned. Peening the weld in steam service has higher risk level especially pressure vessel. In case of low pressure steam service try to arrest the leak with the help of online sealing as a temporary measure, provided its an emergency. Later on as mentioned by Mr. Bapat, go for complete UT and find the leak path.

Sent from Yahoo Mail on Android



From: Ramesh Bapat <rba...@hotmail.com>;
To: <material...@googlegroups.com>;
Subject: [MW:21248] RE: 21247] peening as a temporary repair
Sent: Wed, Jun 25, 2014 2:05:14 AM

veera raghava kommisetti

unread,
Jun 25, 2014, 7:20:23 AM6/25/14
to material...@googlegroups.com
If defect is known, it should be removed completely prior to repair. Superficial repair would be is not a solution. Even if you apply NBIC code (since it is in service), defect has to be removed prior to repair.
 

Ramin Kondori

unread,
Jun 25, 2014, 7:51:57 PM6/25/14
to material...@googlegroups.com
If it is temporary and stops the leak, why not...? go ahead

Best Regards

Ramin Kondori

Sr. QA/QC engineer

Yadavaran Oilfield Project

SIPC (SINOPEC)



--

pgoswami

unread,
Jun 25, 2014, 11:23:45 PM6/25/14
to material...@googlegroups.com, ri...@ritc.co.za
Hi,
 
Those who has access to EPRI, may refer this document for guidance.This document is based on practical experiences on various mock ups. This may work for socket welds or other low pressure lines and would require special peening techniques and special guns.
 
On a "pressure boundary" component like heater the answer is "NO for peening ", whether it's temporary or permanent. The issue is very simple, pinhole leak  could be associated with many many critical  failures if  investigated properly. Failures could be fatal.
 
Weld repair by GTAW would be  best  advisable.
 
Thanks.
 
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 

On-Line Welding Repair for Leaking Pipe Components: Product ID:TR-108132



From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Ramin Kondori
Sent: Wednesday, June 25, 2014 5:01 PM
To: material...@googlegroups.com
Subject: Re: [MW:21258] peening as a temporary repair

Reply all
Reply to author
Forward
0 new messages