ALUMINIUM 6082 -T6

119 views
Skip to first unread message

Vishwas Keskar Welding Manager WELDING

unread,
Aug 22, 2023, 12:00:42 AM8/22/23
to Materials & Welding
Dear Experts 

ALUMINIUM 6082 -T6 - 32mm , 20 mm , 16 mm plates 
32mm ,-32mm- Butt joint
 20 mm-20 mm-Butt joint
16 mm - 16 mm -Butt joint
Above plates are jointed through butt joints  .
Welding Process - GMAW 
Gas - Argon 
Filler wire  - ER4043

Due to job part length , there is distortion at the vicinity of butt welds. So Cold straightening operation was carried out on Press. The weld/HAZ cracking is observed  immediately the press load is commenced

Pl. suggest suitable action for Welding/cold straightening 

Thanks 

Vishwas - IWE





sridhar cn

unread,
Aug 22, 2023, 11:10:59 PM8/22/23
to material...@googlegroups.com
 Aluminium Alloy 6082 has very good weldability, but strength is lowered in the weld zone. When welded to itself, alloy 4043 wire is
 recommended. If welding Aluminium alloy 6082 to 7005, alloy 5356 is used. 

You have not mentioned the parameters selected, tests conducted after welding, or approval standards followed (AWS D 1.2 / 

ISO 15614-2 etc.). Whether NDT (Radiography and visual) or DT (mechanical tests) were carried out before distortion correction.

Pores may create under-bead cracks and potential causes include:

  • Presence of molecular hydrogen.
  • hard microstructure.
  • High weld residual stresses.
  • Fast cooling rate.
  • Not applying preheat or insufficient preheating for welding.

      ·   Welding without cleaning moisture, etc.      

    

During the welding of the Aluminium alloy, hydrogen can cause pores, because its solubility in liquid Aluminium is much higher than 

that in solid Aluminium. Hydrogen is restrained in the molten pool with the advance of the solid-liquid interface. This could be avoided by 

pre-heating the job (due to its high thicknessand causing slow cooling.


Under the stress of external loading, a large number of hydrogen atoms may gather at the grain boundary resulting in stress concentration 

resulting in crack initiation; Under the action of external or tensile stress and a larger stress intensity factor, the poresgenerated by 

hydrogen atom absorption initiates cracks and shows different propagation modes.


Further, due to the higher coefficient of thermal expansion apart from joint pre-heating, avoid continuous welding. Follow sequence welding 

(placing welded metal at different points and joining them together) method, back-step method (to avoid heat concentration), job pre-setting 

(before tack welding) by 5 to 7 deg. etc. to control the distortion.


C Sridhar.

 

·           

 

 


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/597ef31f-53c7-4c81-9924-cbbdd688c49an%40googlegroups.com.

Kannayeram Gnanapandithan

unread,
Aug 23, 2023, 2:23:04 AM8/23/23
to material...@googlegroups.com
u might used 5356 or 5556, 
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


Karthik

unread,
Aug 23, 2023, 3:44:44 AM8/23/23
to material...@googlegroups.com
Hi,
The attached file might be useful to you.

Thanks& Regards,

(Karthik)
Karthikeyan.S
M: +66-892512282
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4ePu3mUEPdaDkyrntUvhFzVN1FkFqCKdND3EjnDqUXCC8g%40mail.gmail.com.

Aluminium alloy welding and fabrication.pdf
Reply all
Reply to author
Forward
0 new messages