We are in the process of manufacturing pressure vessels confirming to ASME Sec VIII. The plate material used is SA 516 Gr.70. The shell thickness is 10mm ad Dished end thickness is 12mm. Do we need to carry out stress relieving of dished end after forming.

Can somebody guide me?

Regards

C G Ravi Shankar

Nunu Nuramanu

unread,
Jun 14, 2011, 7:52:55 AM6/14/11
to material...@googlegroups.com
Hi Ravi,

If I am not mistaken as long as extreme fibre elongation less than 5% & cold forming is used no stress relieve is required. (I did not do design PV for more than 5 years already)

Please check UCS-79 of ASME VIII Div 1 Code for more details.

Hope this helps you.

Regards,

Nunu

Nunu Nuramanu


From: Ravi Shankar <cgr...@gmail.com>
Date: Tue, 14 Jun 2011 15:25:27 +0530
Subject: [MW:11328] PWHT of Dished ends
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

murugesan jeyaraman

unread,
Jun 14, 2011, 10:30:20 AM6/14/11
to material...@googlegroups.com

When the extreme fiber elongation is exceeded by 5% and any one of the following conditions exist a stress relieve is required: I do not remember exactly i think it is UCS 79 of asme sec viii div 1

1) The vessel will contain lethal substances either liquid or gaseous

2) Material requires impact testing
 
3) The thickness of the part before cold forming exceed 5/8".
 
4) The reduction by cold forming from the as-rolled thickness is more than 10% at any location where the extreme fiber elongation exceeds 5%( can not have a min. thickness less than 10% of the nominal thickness to avoid stress relieving if the fiber elongation exceeds 5%)
 
5) The temperature of the material during forming is in the range of 250 Deg F to 900 Deg F.


--

Ramprasad Chari

unread,
Jun 15, 2011, 12:21:54 AM6/15/11
to material...@googlegroups.com
You may go through UCS79 of ASME Section VIII Div 1.Also check tender requirements.Engineers India Ltd, as a standard practice,specifies stress relieving fot thicknesses upto 16mm and Normalising for thicknesses 18mm and above.
Regards
Aarpee

--

jignes...@linde-le.com

unread,
Jun 15, 2011, 3:49:44 AM6/15/11
to material...@googlegroups.com
Dear Mr. Ravi Shankar

 Stress Reliving  of  formed parts is carried ( eg.Dihsed ends) to reduce the stresse developed duirng forming operation / welding.  The applicability of Stress Relieving is based on the following conditions.

1.0 Process Conditions ( eg. Amine services, sour services -)
2.0 Code Requirements ( Refer UCS -79, for your case)
3.0 Project Specifications.

Process conditions will take precedence, evenif expemetd from code requirements.

Check design basis and document precendece order for  applicable documents. Normally, project specifications will take precedence over code requirements.

With Best Regards,

Jignesh R Rana
Manager - Materials Technology, QA/QC & Standards
LINDE


This e-mail is confidential. If you are not the intended recipient, please notify us immediately. You should not disclose its contents to any other person nor use it for any purposes.


Aniket Gupta

unread,
Jun 17, 2011, 11:51:31 AM6/17/11
to material...@googlegroups.com
hi dear

sometimes you need to meet the requirement of client also , check with your client specification. 

On Tue, Jun 14, 2011 at 3:25 PM, Ravi Shankar <cgr...@gmail.com> wrote:

--

lassaad mokrani

unread,
Jun 17, 2011, 1:31:39 PM6/17/11
to material...@googlegroups.com
Yes Mr.Ravi,
Since cold induces strain (up to 5 per cent) resulting in more hardness. So HT is required.
If you vessel design consider NACE MR 0175 as well, then you have to respect:
*Being in annealed/quenched state
*Hardness limits shall be less than 22HRC


 
2011/6/14 Ravi Shankar <cgr...@gmail.com>

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Meilleures salutations

Mokrani Lassaad
00216 20 649 755
http://www.linkedin.com/pub/lassaad-mokrani/16/364/907


















P     Pensez environnement! N'imprimez ce mail que si c'est vraiment nécessaire
Please consider your environmental responsibility before printing this e-mail


This e-mail is confidential and it is intended only for the addressees. Any
review, dissemination, distribution, or copying of this message by persons
or entities other than the intended recipient is prohibited. If you have
received this e-mail in error, kindly notify us immediately by telephone or
e-mail and delete the message from your system. The sender does not accept
liability for any errors or omissions in the contents of this message which
may arise as a result of the e-mail transmission

amje

unread,
Jun 18, 2011, 8:30:10 AM6/18/11
to material...@googlegroups.com
when percentage fiber elongation is more than 5% which heat treatment (normalising or stress relieving) is to be carried out for CARBON STEEL?
whether thickness is criteria?
 
As per EIL specs,normalising is required if thickness is more than 16 mm

Amit Mavai

unread,
Mar 31, 2016, 7:29:55 AM3/31/16
to Materials & Welding
Dear Ravi Shankar,
  If we talk as per code requirement than in sec-VIII Div -1 it is mentioned that if the fiber elongation of formed head if greater than 5% then SR is required & generally below 14mm thk plate fiber elongation comes below 5%.
And if left code than it is client requirement.

Thanks & Regards

Amit Mavi.