Ferrite No 7 to 8

43 views
Skip to first unread message

Vinay Thattey

unread,
May 26, 2020, 1:51:00 AM5/26/20
to material...@googlegroups.com
Dear Friends ;  For some technical reasons the expected ferrite   after completion of circumferential welding for SS to SS ( ASTM-A -240 SS 316 rolled pipe )  is 7 to 8 . We R using 308L / 316 L filler and obtained result is max 5 . pl advice .

Dinesh Somwanshi

unread,
May 26, 2020, 12:30:47 PM5/26/20
to materials-welding
Dear sir, API 582 defines range of FN 5.

Again it's based on fabrication influence on welded part checking.

Regards

Dinesh

On Tue, May 26, 2020, 08:50 Vinay Thattey <vinay....@gmail.com> wrote:
Dear Friends ;  For some technical reasons the expected ferrite   after completion of circumferential welding for SS to SS ( ASTM-A -240 SS 316 rolled pipe )  is 7 to 8 . We R using 308L / 316 L filler and obtained result is max 5 . pl advice .

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CA%2BQ29OgXQ2ATLV_n9N02pM9cxzYKuCpGX0ah9698DdhMVgOPmg%40mail.gmail.com.

Ramin Kondori

unread,
May 29, 2020, 11:46:48 AM5/29/20
to material...@googlegroups.com
You've made a mistake by using 308L filler metal.
Change the WPS and use only 316L filler metal.

Ramin  Kondori
Sr. QA/QC & Welding Engineer
-----------------------------------------------------------
PG-Dip. in Welding Engineering (IWE  AT  0070)
BSc. in Civil Engineering (IUT)
BGAS Painting Inspector
ASNT Level I&II
                        
IIW-Logo-Colour-small


On Tue, May 26, 2020 at 10:20 AM Vinay Thattey <vinay....@gmail.com> wrote:
Dear Friends ;  For some technical reasons the expected ferrite   after completion of circumferential welding for SS to SS ( ASTM-A -240 SS 316 rolled pipe )  is 7 to 8 . We R using 308L / 316 L filler and obtained result is max 5 . pl advice .

--

Vinay Thattey

unread,
May 30, 2020, 1:46:11 AM5/30/20
to material...@googlegroups.com
I understand 316L with higher chrome will result in better ferrite. But specifications calls for 308L.