Nelson curve / hydrogen service

1,702 views
Skip to first unread message

pradip kumar sil

unread,
Aug 4, 2011, 4:02:43 AM8/4/11
to material...@googlegroups.com
Dear everybody,
Can anybody tell me how can select material for hydrogen service AS PER  NELSON CURVE
Regards
Pradip

jignes...@linde-le.com

unread,
Aug 4, 2011, 5:32:51 AM8/4/11
to material...@googlegroups.com
Dear Mr. Pradip,

Original Nelson curve was prepared by G A Nelson in 194, using two parameters;  operating temperature and partial pressure of Hydrogen with respect to HTHA ( High Temperature Hydrogen Attack.) This curve was first published by API in 1970 and then underwent several changes after noticed cases of HTHA.

Presently widely accepted specification against HTHA is API 941.  Fig. 1 of API 941 defines the temperature limits of various materials against partial pressure of Hydrogen.

If Coincident point (temp and pH2) falls above particular material line, then  HTHA is likely to happen for that material for these conditions.

With Best Regards,

Jignesh R Rana
Linde Engineering India Pvt. Ltd.

This e-mail is confidential. If you are not the intended recipient, please notify us immediately. You should not disclose its contents to any other person nor use it for any purposes.


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

pgoswami

unread,
Aug 4, 2011, 11:26:09 PM8/4/11
to material...@googlegroups.com
Dear Mr. Sil,
 
Some additional points on Nelson Diagram and High Temperature Hydrogen service are as follows.
 
Nelson's diagram is the basic building block for good metallurgical design in high temperature hydrogen service. High temperature hydrogen attack (HTHA), or otherwise known as hot hydrogen attack, is a problem which concerns steels operating at elevated temperatures (typically above 400°C) in hydrogen environments, in refinery, petrochemical and other chemical facilities and, also in  high pressure steam boilers.
 
HTHA is the result of hydrogen dissociating and dissolving in the steel, and then reacting with the carbon in solution in the steel to form methane. Methane pressure builds up, forming bubbles or cavities, micro fissures and fissures that may combine to form cracks

High temperature hydrogen can attack steels in two ways:

a. Surface decarburization.

b. Internal decarburization and fissuring.

In order of increasing resistance: carbon steel, C-0.5Mo, Mn-0.5Mo, 1Cr-0.5Mo, 1.25Cr-0.5Mo, 2.25Cr-1Mo, 2.25Cr-1Mo-V, 3Cr-1Mo, 5Cr-0.5Mo and similar steels with variations in chemistry are the materials recommended for HTHA service.For a specific material, HTHA is dependent on temperature, hydrogen partial pressure, time and stress. Service exposure time is cumulative.
 
Use alloy steels with chromium and molybdenum have  increased carbide stability thereby minimizing methane formation. Other carbide stabilizing elements include tungsten and vanadium. 300 Series SS, as well as 5Cr, 9Cr and 12 Cr alloys, are not susceptible to HTHA at conditions normally seen in refinery units.
 
Hope this would clarify your query.If you have any real issues, feel free to share.
 
Thanks.
 
 
 
Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist & Consultant
Ontario,Canada.
Email-pgoswami@sympatico.ca,
 


From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of jignes...@Linde-LE.com
Sent: Thursday, August 04, 2011 5:33 AM
To: material...@googlegroups.com
Subject: Re: [MW:12102] Nelson curve / hydrogen service

zuhad

unread,
Jul 24, 2019, 10:46:52 AM7/24/19
to Materials & Welding
Dear Expert

Could anybody share, how to define or calculate the partial pressure of Hydrogen on the boiler water tube?
Let say my boiler works at steam pressure 180 kg/cm2 (gauge) and 540 deg C, in this condition how to get the partial pressure of hydrogen, to be applied on nelson curve, if the tube using carbon steel material.

Thanks for your help

zuhad


To unsubscribe from this group, send email to material...@googlegroups.com


For more options, visit this group's bolg at


The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--