GMAW- Spray transfer Lack of Side Wall fusion in FPW welds

98 views
Skip to first unread message

MW

unread,
Mar 8, 2017, 8:36:55 AM3/8/17
to Materials & Welding
I have a technical issue with GMAW- Spray transfer process. The wire is 1.2 mm dia. The joint configuration is single bevel butt joint. The weld defect is mostly Lack of Side Wall fusion. The member thickness is 12 mm. All the welds have back chipping and welding. I suggested employing stringer bead technique to improve side wall fusion. But unfortunately, many of the joints are getting rejected in Ut testing. Kindly suggest some techniques/remedy for this problem. Looking forward to your positive feedback. 

Regards, 

Binoj Nair

c sridhar

unread,
Mar 9, 2017, 12:44:52 AM3/9/17
to material...@googlegroups.com
Mr. Nair.
Few more details are required to conclude the reason for the said 
defects. Assuming the position is 1G, pl. provide following info.

1. Amps used for 1.2 mm size wire
2. Voltage selected for the amps.
3. Stick out used.
4. Type of shielding gas and flow rate.

If your parameters are Satisfactory, one of the reason for LF could be 
weld travel speed. Pl. check that aspect also.

1.20 mm size wire will produce more out put and it may be difficult to
control the speed of weld on 12 mm thick plate for certain welders and 
it may also lead to LF.

May be proper parameters selection help to avoid the said problems. 
Alternatively, 1.0 mm may help but let us verify the weld parameters first..

Sridhar. 


From: MW <raghura...@gmail.com>
To: Materials & Welding <material...@googlegroups.com>
Sent: Wednesday, 8 March 2017 7:07 PM
Subject: [MW:26169] GMAW- Spray transfer Lack of Side Wall fusion in FPW welds

I have a technical issue with GMAW- Spray transfer process. The wire is 1.2 mm dia. The joint configuration is single bevel butt joint. The weld defect is mostly Lack of Side Wall fusion. The member thickness is 12 mm. All the welds have back chipping and welding. I suggested employing stringer bead technique to improve side wall fusion. But unfortunately, many of the joints are getting rejected in Ut testing. Kindly suggest some techniques/remedy for this problem. Looking forward to your positive feedback. 

Regards, 

Binoj Nair
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/deb6536a-6834-489f-8f90-80700a42854d%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


Kannayeram Gnanapandithan

unread,
Mar 9, 2017, 12:45:02 AM3/9/17
to materials-welding
What is current &voltage

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

dilintas

unread,
Mar 9, 2017, 11:56:32 PM3/9/17
to material...@googlegroups.com
Make sure that you are not in short circuit mode.
Reduce travel speed.
Work at the higher ampere range.



Sent from my Samsung Galaxy smartphone.

-------- Original message --------
Date: 08/03/2017 16:36 (GMT+03:00)
To: Materials & Welding <material...@googlegroups.com>
Subject: [MW:26169] GMAW- Spray transfer  Lack of Side Wall fusion in FPW welds

I have a technical issue with GMAW- Spray transfer process. The wire is 1.2 mm dia. The joint configuration is single bevel butt joint. The weld defect is mostly Lack of Side Wall fusion. The member thickness is 12 mm. All the welds have back chipping and welding. I suggested employing stringer bead technique to improve side wall fusion. But unfortunately, many of the joints are getting rejected in Ut testing. Kindly suggest some techniques/remedy for this problem. Looking forward to your positive feedback. 

Regards, 

Binoj Nair

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

Chandra

unread,
Mar 9, 2017, 11:56:35 PM3/9/17
to material...@googlegroups.com
Please tell us, which position are you welding?
I will suggest you the welding parametrs for carbon steel gmaw process.

Best Regards,
Chandra
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4ePEFoOJsFSW3ho5Wa1Skw%2BpW6opsM%3D4dG1GrKa%2BvFG4sA%40mail.gmail.com.

binoj nair

unread,
Mar 9, 2017, 11:56:50 PM3/9/17
to Materials & Welding
Ampere range: 140-220 A
Voltage range: 16-28 V

binoj nair

unread,
Mar 10, 2017, 9:36:21 PM3/10/17
to Materials & Welding
Welding Position is 1G i.e. flat

Prashant Panchal

unread,
Mar 10, 2017, 9:36:24 PM3/10/17
to material...@googlegroups.com
Dear chandra sir,
Can you please let me know the parameters for 1.2mm gmaw welding in carbon steel.
Current voltage speed and stickout


Chandra Sekhar

unread,
Mar 10, 2017, 11:27:11 PM3/10/17
to material...@googlegroups.com
Dear SIr,

Please try 
220 - 240 AMps, 
24 - 27 volts
24 to 30 cm/min
10 - 15 mm stick out length 

Sure you will get good results.
We will use this as usual.

Chandra
 

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.

To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.

To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.

To post to this group, send email to materials-welding@googlegroups.com.

Kannayeram Gnanapandithan

unread,
Mar 11, 2017, 1:42:13 AM3/11/17
to materials-welding
for this stick out, u will get only Dip transfer/Globular

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Sat, Mar 11, 2017 at 9:53 AM, Chandra Sekhar <chandrasekh...@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (chandrasekhar.palapala@gmail.com) Add cleanup rule | More info

Dear SIr,

Please try 
220 - 240 AMps, 
24 - 27 volts
24 to 30 cm/min
10 - 15 mm stick out length 

Sure you will get good results.
We will use this as usual.

Chandra
 
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.

To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.

To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.

To post to this group, send email to materials-welding@googlegroups.com.

For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.

To post to this group, send email to materials-welding@googlegroups.com.