Ductile to Brittle Transition Temperature

1,974 views
Skip to first unread message

limesh M

unread,
Aug 10, 2010, 11:21:26 AM8/10/10
to material...@googlegroups.com

Dear All ,

What is DBTT(Ductile to brittle transition temperature)?

How we can find DBTT?

Is there any relationship between DBTT and Drop weight tear test?
 
Regards,
 
 
Limesh

saidulu anthati

unread,
Aug 10, 2010, 1:17:08 PM8/10/10
to material...@googlegroups.com
Dear limesh
 
DBTT
The temperature for which the impact energy is halfway between the impact energy for the highest temperature and the impact energy for the lowest temperature. This definition is usually expressed as the temperature corresponding to the average energy of the upper and lower shelf values.
THE EXPERIMENT

The objective of this experiment is to determine the ductile-brittle transition temperature, Tdt, for the low carbon steel and to give you an appreciation for the large decrease in toughness that occur in certain materials when the temperature is reduced. You will; therefore determine the impact energy for the type of specimen provided, at different temperature. The following temperature baths should be prepared:

Hot water both (about 100 °C)

melting ice (0 °C)

liquid nitrogen (-195.8 °C)

Place two specimens in each bath and allow it to come to the temperature of the bath before testing.

BE VERY CAREFUL WITH THE LIQUID NITROGEN. CONTACT WITH LIQUID NITROGEN OR WITH OBJECTS AT LIQUID NITROGEN TEMPERATURE WILL FREEZE YOUR SKIN INSTANTANEOUSLY AND CAUSE BLISTERS WHICH HEAL VERY SLOWLY.

Move the pendulum of the impact tester to its highest position and ascertain that it is surely locked in this position. Set the plastic pointer to 15 joules (straight down). Now release the pendulum by turning the black knob clockwise.

BE SURE THAT NOTHING, INCLUDING YOUR ARMS AND HANDS, ARE IN THE PATH OF THE PENDULUM. IT CAN EASILY BREAK YOUR ARM!

Stop the pendulum with beak by pushing the red knob up. The pointer on the dial should read zero, because the pendulum will not have lost any of its energy. If it does not read zero contact the TA.

We are now ready to do the actual experiment. The specimens should be transfered from the bath to the anvil as fast as possible, otherwise the temperature of the specimen will change too much (for the low temperatures the specimens will warm up somewhat anyway). Use tongs to transfer the specimen and let the tongs' temperature equilibrate in the bath before removing the specimen. The specimen should be placed on the anvil with its notch on the side opposite where the hammer will hit, and the notch should be in the middle between the supports. Release the pendulum as soon as possible. Read the amount of energy lost in the fracturing process and inspect and describe the fracture surface. The surface should change from dull for ductile fracture, to shiny for brittle fracture. Explain this behavior in your report.

For your report you should plot the impact energy as a function of temperature and draw a smooth curve through your data points. Look at note at bottom of lab for the data. (warning:there may be substantial scatter in your data and you should see a TA if you are not sure how to draw the best curve through your data points). From this curve you should determine Tdt. Several different definitions are used for the transition temperature. We define it as the temperature for which the impact energy is halfway between the impact energy for the highest temperature and the impact energy for the lowest temperature. This definition is usually expressed as the temperature corresponding to the average energy of the upper and lower shelf values.


 


 
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

hpi001

unread,
Aug 10, 2010, 2:18:55 PM8/10/10
to Materials & Welding
DBTT is the temperature at which the fracture surface of charpy-V
impact test samples turns in to brittle and the values drop down.
For determining this temperature you need a lot of charpy specimens
from the same material or weld sample.
You first start to test single specimens at different temperatures
(which temperature depends on the material) in order to find the
temperature range where you need to execute the test and to reduce the
number of specimens needed.
For example for carbon steel you may test a specimen at 0, -40 and -
80 °C. If the specimen at -40 °C already shows a full brittle fracture
surface without any lateral expansion, and at 0 °C the fracture
surface consist both brittle and tough parts it's sure that the DBTT
lays in between these temperatures.
From this point on you need to test sets of 3 specimens, in this case
at for example +20, +10, 0, -10, -20, -30°C. All these values you can
put in a diagram (Impact value against temperature) and will give you
a curve showing a line from 100% brittle fracture to 100% tough
fracture. You will see that you have a specific temperature where the
values drop from constant high values to constant low values.
To determine the exact DBTT you first need to specify this DBTT. Some
specifications say it should be the temperature half way between 100%
tough and 100% brittle, other specifications specify a minimum charpy
value for the DBTT.

The Drop Weight tear test is a test method similar to charpy impact
testing but at which full thickness samples will be tested against
standard 10x10 mm samples for charpy tests.

Hope this answers your question.

Best Regards,

Herman Pieper

ashish chauhan

unread,
Aug 11, 2010, 7:14:07 AM8/11/10
to material...@googlegroups.com
it is the temp below which if use the material , material will fail. suppose one material has DBTT -35C,if we use this material below -35C then its property will change from ductile to brittle and material will fail in brittle manner though it is ductile. drop weight tear test is type of test to measure the DBTT. we can measure DBTT by differene test method like charpy V-notch, drop weight test, explosion bulge test

--

pgoswami

unread,
Aug 11, 2010, 11:08:51 PM8/11/10
to material...@googlegroups.com

Hello Limesh,

In addition to the nice explanations of Mr Herman Pieper, you may find the
attached presentation as useful on DBTT.
There is no specific rule of thumb for DBTT, a lot of factors could
influence this, e.g. composition, melting practices, heat treatment, and the
temperature of charpy impact test.One will need a set of impact test and
plot the values to find the nearest DBTT to the nearest value.

Drop weight test (DWT) typically indicates the nil ductility
temperature(NDT) for any steel under question. It's not commonly asked in
ASME Code.

Only ASME Sec-III code ,Part-NB, NC & ND have requirements of DWT so as to
correlate between DWT and charpy V-Notch testing. For all these codes this
requirement is referenced in NB/NC/ND 2320.

Applicable ASTM spec for DWT is E-208. See the brief illustration about this
test in the attachment.

Thanks.

Pradip Goswami,P.Eng.
Welding & Metallurgical Engineer/Specialist
Ontario Power Generation Inc.
Email-p...@sympatico.ca,
pgos...@quickclic.net

Best Regards,

Herman Pieper

--