WPS - In service welding

455 views
Skip to first unread message

anas k

unread,
Nov 29, 2014, 9:22:30 AM11/29/14
to material...@googlegroups.com
Dear Experts,

I am in a situation to establish WPS for in service piping as per 1104 Annex B. The WPS is for a split tee tie in joint (Encirclement Tee)
Split tee ASTM A 516 Grade B
Header pipe 24" sch 60 (API 5L Grade B)

How to select the thickness range ?
How to select dia range ?
What are the essential variables ?

Please guide me to make a preliminary WPS.

Thanks & Regards
Anas Karanath




Faisal Shahzad Meer

unread,
Nov 30, 2014, 12:35:24 PM11/30/14
to material...@googlegroups.com

Hera are some recommendations to qualify PQR for In service welding of split Tee.

 

·         The requirement for production welding in section 5/7 should be applied to in-service welding except for the additional requirement given in the appendix-B.

·         For circumferential fillet weld Dia, thickness and base metal are not the essential variables as per Appendix B, Para B.2.2.1.1 and 2.2.1.3.(additional requirements) but not for longitudinal groove weld.

·         For in service welding PQR needs to be qualified as per fig B-2.

·         Mechanical test should be as per  Table B-1.

·         C.E and pipe operating conditions shall be mentioned in the procedure.

 

 

Regards

 

Faisal Shahzad Meer

 

cid:image002.jpg@01CCFE94.22F135F0cid:image002.jpg@01CC027E.87D3EED0

TEL :+966 3 6795805-7 Ext. 124|www.gccksa.com

E-mail  fm...@gccksa.com 

Description: MCj03968400000[1]+966 - 553919249

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

joydev dalai

unread,
Nov 30, 2014, 11:56:59 PM11/30/14
to materials-welding

Dear sir,

As per API 1104 the Dia range 

A change from one specified OD group to another. These groups are defined as follows:

1) specified OD less than 2.375 in. (60.3 mm),

2) specified OD from 2.375 in. (60.3 mm) through 12.750 in. (323.9 mm),

3) specified OD greater than 12.750 in. (323.9 mm).

As per API 1104 the thickness range 

A change from one specified wall thickness group to another. These groups are defined as follows:

1) specified pipe wall thickness less than 0.188 in. (4.8 mm),

2) specified pipe wall thickness from 0.188 in. (4.8 mm) through 0.750 in. (19.1 mm),

3) specified pipe wall thickness greater than 0.750 in. (19.1 mm).


anas k

unread,
Dec 1, 2014, 6:05:46 AM12/1/14
to material...@googlegroups.com
Thanks Mr. Faisal and Mr.Joydev.
Is the sections 5/7 is applicable to in service welding ? How we can justify this?

Regards
Anas


Faisal Shahzad Meer

unread,
Dec 2, 2014, 10:42:08 PM12/2/14
to material...@googlegroups.com

MR. ANAS

 

YES

IF YOU WILL GO THROUGH APPENDIX –B  IT CLEARLY GUIDES US THAT IN-SERVICE WELDING PROCEDURE WILL BE BASED ON THE API-1104 PLUS ALTERNATIVE/ADDITIONAL REQUIREMENTS GIVEN IN APPENDIX B.

 

Regards

 

Faisal Shahzad Meer

QA/QC WELDING

0553919249

waqas suleman

unread,
Dec 7, 2014, 10:45:19 PM12/7/14
to material...@googlegroups.com
Dear Faisal,

Can you please advise me how to maintain water flow rate in test coupon during performing PQR.
What should be the arrangement in this regard.

Regards,

Waqas Suleman

Faisal Shahzad Meer

unread,
Dec 8, 2014, 2:59:58 AM12/8/14
to material...@googlegroups.com

Dear Waqas

 

Use the attached test assembly (Figure-B-2) given in appendice-B of API-1104.

Then attached the pump with known flow rate with its “fluid in” nozzle during welding to simulate real welding conditions.

Using water during PQR test will qualify all the flow rates and flow media because water produces severe thermal conditions.

 

 

 

Regards

 

Faisal Shahzad Meer

Project Quality Supervisor-Welding

J-505, Saudi Aramco Wasit Downstream Pipelines Project

 

cid:image002.jpg@01CCFE94.22F135F0cid:image002.jpg@01CC027E.87D3EED0

TEL :+966 3 6795805-7 Ext. 124|www.gccksa.com

E-mail  fm...@gccksa.com 

Description: MCj03968400000[1]+966 - 553919249

 

TEST ASSEMBLY.PNG

Ibraim Ali Elfadol

unread,
Oct 31, 2016, 2:19:12 AM10/31/16
to Materials & Welding, fm...@gccksa.com
Dear Waqas

السلام عليكم ورحمة الله

Please advise us about the following
1. We are preparing a new WPS for in-service welding.
2. Our scope is mechanical sleeve type b pipeline repair.
3. The pipeline operation condition has several flow rates.

do we need to make individual WPS for each flow rate, or one WPS could be applicable for all the flow rates?

Thanks,,,

Ibrahim Ali Elfadol Mohammed
Construction Manager
EXICO Petroleum Services Co.
eng.i...@gmail.com
+249126466109

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com


For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.


For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com


For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.


For more options, visit https://groups.google.com/d/optout.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com


For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.


For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com


For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.


For more options, visit https://groups.google.com/d/optout.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com


For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.

Reply all
Reply to author
Forward
0 new messages