Required details of the equivalent ASME Grade for EN1.4306 or EN1.4307

34 views
Skip to first unread message

dham...@gmail.com

unread,
Sep 30, 2026, 1:07:24 AM (5 days ago) Sep 30
to Materials & Welding
Hello Team,

Request to provide details of the equivalent ASME Grade for EN1.4306 or EN1.4307.

Also i had try to down EN specification from the authorized portal but unable to find the mother specification for these grades. 

Thanks & Regards,
Dharmesh Mistry

Kannayeram Gnanapandithan

unread,
Sep 30, 2026, 1:40:27 AM (5 days ago) Sep 30
to material...@googlegroups.com
ss304
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015, ISO 3834, EN 1090 & EN 15085, 
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/f75745db-ff16-4970-a9c3-99d3cc20e550n%40googlegroups.com.

K Dinesh

unread,
Sep 30, 2026, 1:40:31 AM (5 days ago) Sep 30
to material...@googlegroups.com
Hi,

PFA.

image.png

Thanks & Regards

K.Dinesh 

Metallurgist


P.O. Box 1197, P.C 130, Muscat, Sultanate of Oman

Tel:  +968 24501524, 24505590 (Ext.53), Mob: +968 99880633, Fax: +968 24503814

Email: dinesh@lonestaralpha.com , Web: www.lonestaralpha.com , Location: Click here for Location Map

Locations: Muscat, Sohar, Duqm, Salalah & Liwa

Lonestar now does Pesticide Residues Testing in our new facility at Liwa!

 Consider your environmental responsibility. Think before you print.



--

dham...@gmail.com

unread,
Sep 30, 2026, 2:30:50 AM (5 days ago) Sep 30
to Materials & Welding
Hi all,

Query was "this grade (EN1.4306 or EN1.4307) under which EN specifications". 

Regards,
Dharmesh

Bhavani Prasad Emani

unread,
Sep 30, 2026, 6:46:06 AM (5 days ago) Sep 30
to material...@googlegroups.com, dham...@gmail.com
Hi,
Both EN 1.4306 (X2CrNi19-11) and EN 1.4307 (X2CrNi18-9) are commonly cross-referenced to ASME/ASTM Type 304L, UNS S30403. Grade equivalence alone does not establish ASME Code compliance: the applicable specification depends on the product form. For example, plate, sheet, or strip may use SA-240 Type 304L, while pipe may use SA-312 TP304L. Verify the material against the specification and Code edition required for the application.


Thanking you,

With best regards,                                            
           
Bhavani Prasad Emani,
Associated Engineering Services
#3-5-944/205-206 & 220-221,
2nd Floor, Panchavati Mall,
Narayanaguda, Hyderabad, India.
Mob.No: +91 9032585485
Website: www.aesinspections.in,
Email: in...@aesinspections.in

     This email and any attachments may contain confidential or legally protected information intended only for the named recipients. If you received this in error, please notify the sender immediately and delete it. Unauthorized use, copying, or distribution is prohibited.




--

sridhar cn

unread,
Oct 4, 2026, 8:14:25 AM (yesterday) Oct 4
to material...@googlegroups.com

 EN no.

        EN design.

      Common name

      Closest ASME/

   ASTM grade

Key distinction

1.4306

       X2CrNi19-11

             304L 

       SA-240 Type 304L

          Higher Cr/Ni than 1.4307; very low C

1.4307

       X2CrNi18-9

             304L

       SA-240 Type 304L

          Standard 304L composition

 

Sridhar.


Reply all