Radiography for Forged valve

217 views
Skip to first unread message

nasrath ali

unread,
Dec 6, 2023, 10:23:26 AM12/6/23
to Materials & Welding

Dear All,

As per API 6D, testing for Valves, Code does not call for Radiography Testing for Forged Valves, whereas RT is mandatory for Cast Valves.

Kindly clarify the reason for not stipulating RT on Forged Valve

Thanks.

MRTEJS1

unread,
Dec 8, 2023, 9:58:26 AM12/8/23
to material...@googlegroups.com
Dear 

Understand what type of defects in both different materials,then you understand why specific requirements of UT or RT


Tejas 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/31f196c7-0051-4151-ae91-b902c77f0789n%40googlegroups.com.

james gerald

unread,
Dec 8, 2023, 9:58:26 AM12/8/23
to material...@googlegroups.com
There are some differences between Cast & Forged products.

CAST VALVE                                                                             FORGED VALVE
1. Castings are normally associated                                          1. Except Hot shortness not much defects in
    with defects and Inclusions which                                               Forgings which can be controlled.
     affect the Integrity of the valve

2.  Normally no Heat Treatment after castings                           2. Forgings receives Grain refining Heat 
                                                                                                        Treatment and better rpoperties.

3. No limitation on Sizes of Valves                                             3. Only smaller sizes mostly

4. Low cost                                                                                 4. Higher cost


RT is specified only to Cast valves because it is prone to Defects like Porosities & inclusion.

Thanks & Regards

J.Gerald Jayakumar



--

nasrath ali

unread,
Dec 18, 2023, 3:51:20 AM12/18/23
to material...@googlegroups.com
Dear Mr. Gerald,

Appreciate your response. It was helpful.

Thanks.