I am working in pipeline project API1104.
I heve one speciemen breaks on the weld in tension test for mechanized welding operator with filler metal and the tension strength was greater the SMTS.

 pls advise what we should do in this case?
ahmed

meisam shokri arfaei

non lue,
8 nov. 2015, 04:57:1708/11/2015
à material...@googlegroups.com
Hi

There is nothing to do. The test is accepted.

Regards

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/94f6694b-637f-4cbf-a89e-eac19f4910d0%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.



--
M. Shokri Arfaei
ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer





Vishwas Keskar Welding Manager Pune India

non lue,
30 nov. 2015, 22:28:5630/11/2015
à Materials & Welding
if the breaking  tensile strength is more than the base metal, then no problem
In PQR , write that "Fracture in Weld "
that's all

Kannayeram Gnanapandithan

non lue,
1 déc. 2015, 22:42:4601/12/2015
à materials-welding
As per API 1104, in addition to tensile strength ( If breaks in weld with strength greater than base metal), u have to check the requirement of soundness of weld. say gas pocket should not be greater than 1.6mm, slag inclusion less than .8, in depth, and not more than 3mm or one half the nominal wall thickness in length. atleast 13mm separation in between slag, if above requirments  are met, then it is acceptable

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
Répondre à tous
Répondre à l'auteur
Transférer
0 nouveau message