Set On Nozzle - Governing thickness for WPS

825 views
Skip to first unread message

Chintan Raval

unread,
Jan 5, 2023, 3:53:49 AM1/5/23
to material...@googlegroups.com
Dear Expert,

Kindly advice,

For Pressure Vessel as per ASME Sec 8 Div 1,

Nozzle to Shell full penetration weld of Set on type nozzle, which is the governing thickness for wps selection i.e. thickness of nozzle or thickness of shell or both.

In a typical case,

Nozzle thickness 14 mm, needs to be welded on another nozzle of thickness 250 mm.

WPs available is with 5 mm to 200 mm range.

Is this wps can be used for set on type nozzle as it cover range of nozzle thickness

Sourav Bohrays

unread,
Jan 5, 2023, 10:25:36 PM1/5/23
to material...@googlegroups.com
No
250 is governing thickness

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOdsS43ZLNQgO-s0Am8pQw5bJHg2X8SZBSTaZJXTy0zytLymFA%40mail.gmail.com.

Jenish Mistry

unread,
Jan 5, 2023, 10:25:37 PM1/5/23
to material...@googlegroups.com
Governing Thickness : 14 mm.

--

james gerald

unread,
Jan 5, 2023, 10:25:38 PM1/5/23
to material...@googlegroups.com
Yes this WPS can be used provided PQR qualified on thickness 38mm and higher,

Please see below some snap shots of Sec.IX.

Inline image

Inline image


Please see snap shot of ASME Sec8 Div.i for Nozzle connections

Inline image
Inline image
Inline image

Inline image



Thanks & Regards

J.Gerald Jayakumar




--

Kannayeram Gnanapandithan

unread,
Jan 5, 2023, 11:01:22 PM1/5/23
to material...@googlegroups.com
Set in, Set on , the governing thickness is nozzle^s thickness, if it is set through ,then it is Header thickness

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


Sourav Bohrays

unread,
Jan 6, 2023, 3:31:12 AM1/6/23
to material...@googlegroups.com
Dear 
Please share weld design or figure for weld joint including both pipe

On Thu, 5 Jan 2023, 12:53 pm Chintan Raval, <chin...@gmail.com> wrote:
--

Sourav Bohrays

unread,
Jan 6, 2023, 6:53:22 AM1/6/23
to material...@googlegroups.com
Dear chintan

Ignore my previous reply.
1.if nozzle is fitup like seton and  bevel in only seton nozzle not in branch(pipe,plate) than governing thickness will be seton on noozle not branch(pipe,plate).

Reason- welding to be done around seton nozzle with whatever fillet require.

2. If noozle is fitup like seton and bevel in only branch(plate,pipe) than governing thickness will branch thickness

Reason- in this case welding to be filled in bevel of branch so  branch thickness  will be the mandatory thickness for wps.


3.if noozle and branch both has bevel and seton noozle fitup on branch than whichever is maximum thickness will be mandatory thickness