Hi Everyone,

We have encountered as PQR for Inconel-625 WOL on SA516 Grade 70 Normalized plate in 3G position.

Two Anomalies were observed: 
1. After PWHT of 120 mins, Hardness in base metal dropped from average 164 HV to average 108 HV! Has anyone observed such a drop in hardness? Is it possible? 
2. 625 WOL is done using SMAW electrode from Special Metals, the Nickel content as per consumable TC is 65%. While in WOL chemistry, 1.5mm from Top, Nickel % came around 68%. 3% Higher!! Is this possible, in any case?

Thanks in advance from your expert views.

Regards,
Mohammed Dudhiyawala, IWE

Mohd Siraj

unread,
Oct 22, 2025, 12:40:52 PM10/22/25
to Materials & Welding
dear mohd,

1. what was base metal thickness? is PWHT done to qualified for two PWHT cycle?, 
      # hardness achieved  after pwht100-140 hv is normal.

2. if Nickle 68% is concern, try with GTAW process.

Mohmmed Dudhiyawala

unread,
Oct 27, 2025, 12:39:34 AM10/27/25
to Materials & Welding
Base metal thickness is 5mm & deposited WOL is also 5mm.
Hardness achieved is after PWHT 1 Cycle of 60 mins.