Dear Experts,
We are facing problem of leakage during service condition in heat exchanger. Leakage are coming in the tube to tube sheet welding in service condition. Attached are the reference photos
Details are defined below,
Construction code – ASME SEC-VIII Div-1 and Div-2
Material – Tube Sheet - SA 240 UNS 31803
Tube - SA789 UNS 31803
Filler – ER2209
Allowable Temperature – Shell – +180 / -30 C, Pressure- 1 bar /FV
Allowable Temperature- Tube- +200 /+10 C, Pressure 10 bar
MDMT -0 C
Service Media – Shell – Methanol + LIBR
Tube – Thermal oil
Let us know why such failure occurs and preventive actions
Dear Chandan Sharma,
The leaks in your tube bundle appears to be from the cracks in the Tube/Tube sheet welds. Please look at your fabrication details for the tube bundle. The cracking could be caused by the expansion of the tubes while in service.
A thorough investigation into the Manufacturing process will be needed before attempting a repair procedure.
Regards
George V Aliyattukudy
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-weld...@googlegroups.com.
To post to this group, send email to
material...@googlegroups.com.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/CAHTWUJL8WSL77tHp8HGSVH7pYZfm4Oe3-xzmBHntE3n5aaKpYQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b649727e-a05c-4bf4-976e-ffd26a8c65d0%40googlegroups.com.