Hi,

I am seeking insights from anyone who has experience meeting the 0.015 in. lateral expansion requirement for full-size Charpy V-notch tests at -320°F for SAW SS316L welds, as outlined in UHA 51 of ASME Section VIII, Division 1-2025. The base metal is SA 240 Type 316L, which has been solution annealed prior to welding and is 1.50 in. thick.

If you have relevant experience, I would greatly appreciate it if you could provide details on the following aspects:

  1. The impact of using more passes versus fewer passes,

  2. The comparison between square wave AC and DCEP,

  3. The maximum heat input utilized,

  4. The effects of low delta ferrite (2-5 FN) in the weld versus Creq/Nieq ratios (<1.48 or >1.95),

  5. Solidification modes observed (e.g., F to A, A to F),

  6. The morphology of ferrite (e.g., vermicular or lathy),

  7. The cooling rate (still, air, or water-cooled),

  8. Any metallographic observations related to the formation of M23C6 or sigma phase,

  9. Any additional observations related to crystallography or texture.

Thank you for your assistance.

Best regards,

Sandeep Singh Parmar
Materials & Welding Expert
SGS Canada Inc.



Vishwas Keskar

unread,
Jun 1, 2026, 12:12:27 PMJun 1
to material...@googlegroups.com
Which flux wire you are planning for 

Vishwas 
IWE

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/c1dff320-75f4-49dc-ba41-ec53818bcd58n%40googlegroups.com.

Sandeep Singh Parmar

unread,
Jun 1, 2026, 1:26:31 PMJun 1
to Materials & Welding
Hi, the plan is to use wire and flux made by Boehler, of the matching chemical compositions. 

Thanks
Sandeep
Welding and Materials Expert.

Vishwas Keskar

unread,
Jun 1, 2026, 2:03:13 PMJun 1
to material...@googlegroups.com
Great 
As I recall they have typical a low ferrite , High Ni wire / flux that  gives you consistent LE  values .
Also EXATON FLux wire also are consistent 
Check that flux with High basicity index EXATON 50W 
Run PQR and ensure LE  values are achieved .

atul jha

unread,
Jun 1, 2026, 2:21:46 PMJun 1
to material...@googlegroups.com
  1. The impact of using more passes versus fewer passes, ---Each Pass Thickness should not be more han 2.5 mm

  2. The comparison between square wave AC and DCEP,  use Lincoln 1000-SD ( Hope you understand if you have this machine) 

  3. The maximum heat input utilized-- For SAW welding Limiting Value 2.5 KJ/mm ( Note: Don't keep Heat Input below 1.5KJ/mm)

  4. The effects of low delta ferrite (2-5 FN) in the weld versus Creq/Nieq ratios (<1.48 or >1.95), ( Nippon Steel SAW wire & Flux BEST IN CLASS Convey this to them through TDC , THE R & D Team will take care, and on the shop floor you will not face any issue.

  5. Solidification modes observed (e.g., F to A, A to F), It will be FA Mode.

  6. The morphology of ferrite (e.g., vermicular or lathy), ( Why are you interested in It? Please share. It's a research Work or a shop floor job 

  7. The cooling rate (still, air, or water-cooled), Normal Cooling Still Air IP should be less than 175 OC.

  8. Any metallographic observations related to the formation of M23C6 or sigma phase? No sigma in weld if wire is from Nippon ( I don't have any commercial interest in Nippon, but this wire & flux is best in class, miles ahead of any other, & R & D support is awesome.

  1. Any additional observations related to crystallography or texture.

    Thank y


    Mohd Siraj

    unread,
    Jun 29, 2026, 9:08:33 AMJun 29
    to Materials & Welding

    Given the difficulty in finding someone with direct experience matching this exact situation, 

    I suggest,

    Design and run a single, well-instrumented PQR

    Coordinate closely with leading filler metal manufacturers.