Request for Information

69 views
Skip to first unread message

G Gughan

unread,
Jan 12, 2023, 3:19:57 AM1/12/23
to material...@googlegroups.com
Dear Experts,

It's a very nice platform to gain & share knowledge.

I have a query regarding the weld bead length. What is the maximum weld bead/weave length in Power Piping? (ASME B 31.1)
or 
Is there any thumb rule for weld bead length?

Your idea/advice will be highly welcomed & appreciated.

Be safe & have a healthy Life

Thanks,

Kind Regards,

G.Gughan

Babur Khan

unread,
Jan 12, 2023, 4:48:07 AM1/12/23
to material...@googlegroups.com
Greetings,
Weld bead width or length? 

Muhammad Babur Khan
Sent from my iPhone

On 12 Jan 2023, at 11:19 AM, G Gughan <ggug...@gmail.com> wrote:


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAB0bcTMUzgWi-7pQvfdjj-e93ChHhYcq93UYgWC3xe9Kv4hnng%40mail.gmail.com.

Vishwas Keskar Welding Manager WELDING

unread,
Jan 13, 2023, 1:44:22 AM1/13/23
to Materials & Welding
it seems the query is related to Weaving Technique !
So responce is as below 
For SMAW -
The Engineer shall address weaving width in WPS.
In general , weaving is permitted up to 3-4 Times the core diameter of the electrodes.

You may write WPS addressing as :
Root pass and Hot pass - Stringer bead technique
Fill up passes - Weaving Technique -  Maximum 6 Times   the core diameter of the electrodes.

This is in general  rule
Contract/Bid/Specification document shall  prevail over Normally followed weaving rules

Thanks and regards

Vishwas -IWE
International Welding Engineer 

G Gughan

unread,
Jan 13, 2023, 1:44:23 AM1/13/23
to material...@googlegroups.com

GENE MATSKO

unread,
Jan 13, 2023, 1:44:23 AM1/13/23
to material...@googlegroups.com

james gerald

unread,
Jan 14, 2023, 7:20:18 AM1/14/23
to material...@googlegroups.com
Use of string / Weave weld bead according to ASME Sec.IX is considered non essential variable which is considered as the requirement of ASME B31.1.

See below snap shot.

Inline image
Inline image



But Client Specification will have control over the Bead width. For eg see snapshot

Inline image

Some consumable Manufacturer's Welding Handbook's also provides some guidance.

Normally Weaving will have an effect on the below.

1. Weld pool control depending on the Fluidity of weld liquid metal.
2. For low temperature metals will have an effect on the Charpy Impact properties as Weave width increases the Travel speed will be low and hence the Heat Input will be higher which reduces the cooling rate and hence aids in coarsening of grains and hence the charpy Impact properties.
3. Will have a problem in positional welding.

Thanks & Regards

J.Gerald Jayakumar