Dear Community Members.

We have done a PQR coupon for welding Weldox 700E. The material Thickness was 35 mm. Double V Groove Butt Joint. 2G position. Code AWS D1.1

The following parameters were followed

Process = FCAW
Electrode wire = Esab Dual Shield II 110 
Gas = 80 % Argon 20% Co2
Gas Flow = 20 lpm

Preheat to 103 C
Interpass temp around 150 C

Current Settings 

DCEP CV
Amps 200 amps 24 Volts for root pass 
Amps 180 to 160  24 Volts for hot, fill and capping.

The heat input recorded was between .8 to 1.5 kj/mm
The wire feed rate was 10 m/min

We did a charpy test on weld metal however it failed.
The results were average of 8 kj absorption at -40 C

At 1mm and 5mm from fusion line the absorption was 80 to 130kj

Intend to do a re charpy test @ -18 C.

Though the client has not specified Charpy requirements and specifications. Wanted to do it for future requirements if any.

Request you to please share your opinion,

WHAT COULD BE THE REASON THE CHARPY @ WELD METAL IS SO LOW, and in the absence of specific requirements for CVN what should be the impact values.

AWS D1.1 does not state any values for Yield strength above 355 MPA, but leaves the onus on the client to specifiy.

Please advise.

Thanks
Rudolf




kannayeram gnanapandithan

unread,
Jun 16, 2013, 2:42:04 AM6/16/13
to materials-welding
This attachment may be usefull 


Rudolf




--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Welding_HARDOX_and_WELDOX[1].pdf

J Prinsen

unread,
Jun 17, 2013, 4:37:42 AM6/17/13
to material...@googlegroups.com
What were the original impact values of the base metal

Jurgen Prinsen IWE

----- Oorspronkelijk bericht -----
Van: "kannayeram gnanapandithan" <kgpan...@gmail.com>
Aan: "materials-welding" <material...@googlegroups.com>
Verzonden: Zondag 16 juni 2013 08:42:04
Onderwerp: Re: [MW:17941] PQR for Welding Weldox 700

Rudolf

unread,
Jun 17, 2013, 4:42:27 AM6/17/13
to material...@googlegroups.com, material...@googlegroups.com
Average of 165 joules

Sent from my iPhone

J Prinsen

unread,
Jun 17, 2013, 5:52:37 AM6/17/13
to material...@googlegroups.com
Did yoy secure the fit-up tight enough.
If you give the testplate room for free deformation, you'll get "strain aging", precipitation at dislocation areas, very bad for impact values.
Use 4 - 5 stiffeners on the back side of the test weld on 40 cm weldlength, first (allmost) completely weld on the front side, then place stiffeners on the front side, remove stiffeners on the back side, clean the backside of the root, and finalize the back weld
After complete cool-down, remove the stiffeners

p.s. Use stiffeners of 35 mm thick, at least 300 mm long, 80 mm high, connect them with fillet welds, z=15 mm to the test plates
Regards

Jurgen Prinsen, MSc, IWE

(experience is learning from mistakes, if you have a lot of experience, you have made a lot of mistakes)
You have cheap experience, you have expensive experience, the expensie one is, when you learn from your own mistakes, the cheap one is when you learn from somebody elses mistakes
If you make no mistakes you often make nothing at all


----- Oorspronkelijk bericht -----
Van: "Rudolf" <rudol...@yahoo.com>
Aan: material...@googlegroups.com
Cc: material...@googlegroups.com
Verzonden: Maandag 17 juni 2013 10:42:27
Onderwerp: Re: [MW:17945] PQR for Welding Weldox 700

rudolf saldanha

unread,
Jun 17, 2013, 7:26:57 AM6/17/13
to material...@googlegroups.com
Hi, Mr. Prinsen,

Fit up was good, in the sense, root face, root gap, but there were only two stiffners given on the back side. I did not think in this angle, that insufficient stiffners could be a cause for bad impact values. Thanks for your advise.

As mentioned earlier I did a test at -18 C, but the results were -9 Joules average, where as there has been a good result in the 1mm and 5 mm fusion line, somewhere around 170 joules.

If I were to try another test plate, surely will follow your advise.

However, could it be due to very low heat input and rapid cooling due to higher thickness, which has resulted in a hard microstructure. 
There were no heating element involved. The interpass temp was measured at 3 inches away from the fusion line.

Thanks 
Rudolf


From: J Prinsen <weld...@online.nl>
To: material...@googlegroups.com
Sent: Monday, 17 June 2013, 17:52
Subject: Re: [MW:17947] PQR for Welding Weldox 700
> To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com
> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsub...@googlegroups.com .
> For more options, visit https://groups.google.com/groups/opt_out .


>
>
>
> --
> To post to this group, send email to material...@googlegroups.com
> To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com
> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsub...@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out .


>
> --
> To post to this group, send email to material...@googlegroups.com
> To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com

> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsub...@googlegroups.com.

> For more options, visit https://groups.google.com/groups/opt_out.
>
>

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsub...@googlegroups.com.

For more options, visit https://groups.google.com/groups/opt_out.


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsub...@googlegroups.com.

Ramin Kondori

unread,
Jun 18, 2013, 2:03:47 AM6/18/13
to material...@googlegroups.com
Dear Rudolf:

Of course it will fail...
This is a Q&T steel...
Along with heat input control, a 35 mm Thick Weldox-700 plate shall definitely require stress relief after welding.

But be careful...
The holding temp shall not exceed that of base metal during manufacturing.
do not apply stress relieve at 600, 620 or so...
Check the plate certificate and you will find the heat treatment parameters there, the PWHT temp shall not exceed the tempering temperature of your weldox-700 plate.

Try to keep heat input around 1.0 KJ/mm. Lower heat input is better.

You are using FCAW...
Not saying that it is wrong but sometimes in Q&T steels, you have to use pulsed arc or spray transfer to get good impact results and for this reason, MIG works better (in case you failed with FCAW).

Good Luck
Ramin Kondori
Sr. QA/QC Engineer
SINOPEC

r.ko...@petroyada.com
+98-2123592322
+98-9132150320



Rudolf




--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

Rudolf

unread,
Jun 18, 2013, 3:18:00 AM6/18/13
to material...@googlegroups.com, material...@googlegroups.com
Dear Mr. Ramin

Thanks for your valuable feed back. But am afraid I have checked with SSAB manufacturer of this plate and am told that PWHT is not mandatory unless the design calls for. 

However I agree with you regarding the transfer method.
The heat input has been very low as the welding speed was good, but. This too fast may also be the reason for insufficient slag covering over the weld puddle and exposure to atmosphere. 

Another possibility may be the low heat input the heat has immediately dissipated to the base metal and the plate has served as a heat sink thereby leading to a hard micro structure. 



Regards
Rudolf

Sent from my iPhone

Ramin Kondori

unread,
Jun 18, 2013, 4:51:23 AM6/18/13
to material...@googlegroups.com
Dear Rudolf:

Are you saying that your specimens did not fail in HAZ (or fusion line) and weld metal specimens failed...?

If "weld metal" impact test has failed, most probably it has something to do either with your filler metal or welding process (or power source settings, technique etc.).

Are you using recommended welding parameters...?
Please check with the ESAB page to ensure you are using proper power source settings (http://www.esabna.com/us/en/products_catalog.cfm?Product_ID=265).

Normally, the problem with welding of Quench & Tempered steels like Weldox-700 is that impact toughness drops in HAZ (and/or fusion line). Of course that's when you select suitable filler metal and welding process and technique. Below table shows that you should not have any problem with weld metal specimens. In other words if you use recommended parameters, you should get these results (for weld metal only). If you have not, then you are missing something.

Typical Mechanical Properties (Weld Metal)

As Welded 75% Ar / 25% CO2

Yield Strength: 110 ksi, 760 MPa
Tensile Strength: 120 ksi, 830 MPa
Reduction in Area: 54%
Elongation in 2": 19%

Stress Relieved 8 hrs. @ 1150°F (621°C) 75% Ar / 25% CO2

Yield Strength: 108 ksi, 745 MPa
Tensile Strength: 116 ksi, 800 MPa
Reduction in Area: 56%
Elongation in 2": 19%

Charpy V-Notch Properties (Weld Metal)

Testing Temperature 0°F (-18°C)

As Welded 75% Ar / 25% CO2 : 40 ft-lb, 54 J
Stress Relieved 8 hrs. @ 1150°F (621°C): 29 ft-lb, 39 J

Testing Temperature -20°F (-29°C)

As Welded 75% Ar / 25% CO2 : 36 ft-lb, 49 J
Stress Relieved 8 hrs. @ 1150°F (621°C) : 27 ft-lb, 37 J

Testing Temperature -60°F (-51°C)

As Welded 75% Ar / 25% CO2 : 26 ft-lb, 35 J
Stress Relieved 8 hrs. @ 1150°F (621°C) : 21 ft-lb, 28 J


That was about "weld metal" but HAZ is another issue here.
PWHT is necessary since it will restore toughness of the HAZ. I don't know why that manufacturer has told you that PWHT is not mandatory. When you have impact requirements, PWHT is essential for restoring toughness in HAZ of QT steels.

I have seen this issue before and by changing the process to Pulsed GMAW the problem solved.
Pulsed GMAW lowers the heat input and you have more control on transfer mode.
I recommend you to do the same. 

Good Luck
Ramin Kondori
Sr. QA/QC Engineer
SINOPEC

r.ko...@petroyada.com
+98-2123592322
+98-9132150320



Rudolf

unread,
Jun 18, 2013, 6:26:53 AM6/18/13
to material...@googlegroups.com, material...@googlegroups.com
Hi Ramin, 
Thanks for your reply. Yes you are right the impact values at 1mm and 5 mm at fusion line is over 150 joules. It is only at the weld metal that it has dropped to single digit. The hardness at root pass weld metal and HAZ is around 350 to 400 HV. The parameters are all fine. Checked with Esab. 
The parameters are given in my first query. 

Am really confused. Why and how it has happened. I have religiously monitored the inter pass temp with temp stick and digital thermometer. Continuously checked V and A using tong meter. Checked gas flow at regulator. 

Thanks and regards 
Rudolf 

Sent from my iPhone

Ramin Kondori

unread,
Jun 18, 2013, 7:50:27 AM6/18/13
to material...@googlegroups.com
Dear Rudolf:

Now that's the information I needed.
At the beginning I thought you have the usual HAZ toughness problem but this one is different.

There are a few reasons for such high hardness values in root pass, including:
  • Alloying elements in this filler metal (1.75% Ni and 2.0% Mn) 
  • Your thickness is 35mm so heat sink is high
  • Root pass geometry causes stress concentration
That means you have to increase Heat input and/or preheat.
But you can't increase preheat so much otherwise you will jeopardize HAZ toughness so PWHT will be essential. There is no other way...!!!

I recommend include back gouging (grinding is better) in your WPS (if you have access in the actual work). Gouging shall be done with low heat input, followed by grinding.
This is to remove this problematic root pass.

Good Luck
Ramin Kondori
Sr. QA/QC Engineer
SINOPEC

r.ko...@petroyada.com
+98-2123592322
+98-9132150320



rudolf saldanha

unread,
Jun 19, 2013, 12:25:18 AM6/19/13
to material...@googlegroups.com
Hi, Ramin
 
Thank you very much for your valuable feed back. I have included Back gouging in the WPS, although this was not done on the WPQT coupon, as the fit up and penetration was excellent, just did back grinding instead of gouging.
 
As suggested, PWHT may be the only solution out.
 
Root pass geometry was Double V 2/3 - 1/3 Bevelling 60 deg. with 3 mm root gap and 2 mm face.
 
Thanks again,
Regards
Rudolf


Good Luck
Good Luck
To unsubscribe from this group, send email to mailto:materials-welding%2Bunsu...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to mailto:materials-welding%2Bunsu...@googlegroups.com.

For more options, visit https://groups.google.com/groups/opt_out.
 
 
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to mailto:materials-welding%2Bunsu...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to mailto:materials-welding%2Bunsu...@googlegroups.com.

For more options, visit https://groups.google.com/groups/opt_out.
 
 
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to mailto:materials-welding%2Bunsu...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to mailto:materials-welding%2Bunsu...@googlegroups.com.

For more options, visit https://groups.google.com/groups/opt_out.
 
 

Ramin Kondori

unread,
Jun 19, 2013, 2:24:05 AM6/19/13
to material...@googlegroups.com
Dear Rudolf

Any time...
Again, If the root pass is the problem, you either change the parameters to achieve desired properties (hardness, impact etc.) or you simply grind out that bloody root pass and proceed.

Personally, I would rather choose the first option. Applying a combination of 150-200C pre-heat, controlled heat input and PWHT (holding temp not higher than base metal tempering temperature) is a routine solution.

If you decided to go for root pass removal, just do not forget to be critical. The gouging heat input shall be kept to minimum and gouging products shall be completely removed by grinding (high-carbon metal or gouging HAZ).

Regards
Ramin Kondori
Sr. QA/QC Engineer
SINOPEC

r.ko...@petroyada.com
+98-2123592322
+98-9132150320



Reply all
Reply to author
Forward
0 new messages