Suitable electrodes for joining AISI 4130

584 views
Skip to first unread message

Pawan Pal

unread,
Nov 12, 2016, 5:17:05 AM11/12/16
to Materials & Welding
Dear Sir,
Thank you for your time to read my question.
 
I want to know which welding electrode is suitable for welding these base metals together  grade AISI 4130 with AISI 4130.
 

 

 
Thanks
 
PAWAN PAL

c sridhar

unread,
Nov 12, 2016, 9:56:18 PM11/12/16
to material...@googlegroups.com
For welding 4130 to 4130,

1. In SMAW process, you can use E 10016-D2 or E 10018-D2.

2. In TIG process it is ER 80 S-D2

Sridhar.



From: Pawan Pal <pawan...@gmail.com>
To: Materials & Welding <material...@googlegroups.com>
Sent: Saturday, 12 November 2016 3:03 PM
Subject: [MW:25667] Suitable electrodes for joining AISI 4130

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/9cc3bd71-800c-4edc-82d4-059d20873f5f%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


George Dilintas

unread,
Nov 13, 2016, 9:20:56 PM11/13/16
to Meghanadh K
In some aerospace and motor applications also ER70S-D2 are used

2016-11-12 18:42 GMT+02:00 'c sridhar' via Materials & Welding <material...@googlegroups.com>:
For welding 4130 to 4130,

1. In SMAW process, you can use E 10016-D2 or E 10018-D2.

2. In TIG process it is ER 80 S-D2

Sridhar.



From: Pawan Pal <pawan...@gmail.com>
To: Materials & Welding <materials-welding@googlegroups.com>
Sent: Saturday, 12 November 2016 3:03 PM
Subject: [MW:25667] Suitable electrodes for joining AISI 4130
Dear Sir,
Thank you for your time to read my question.
 
I want to know which welding electrode is suitable for welding these base metals together  grade AISI 4130 with AISI 4130.
 

 

 
Thanks
 
PAWAN PAL

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/280940935.2724416.1478968951310%40mail.yahoo.com.

For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

Kannayeram Gnanapandithan

unread,
Nov 14, 2016, 12:36:43 AM11/14/16
to materials-welding
ER 70S-A1

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Mon, Nov 14, 2016 at 1:12 AM, George Dilintas <dili...@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (dili...@gmail.com) Add cleanup rule | More info

In some aerospace and motor applications also ER70S-D2 are used
2016-11-12 18:42 GMT+02:00 'c sridhar' via Materials & Welding <materials-welding@googlegroups.com>:
For welding 4130 to 4130,

1. In SMAW process, you can use E 10016-D2 or E 10018-D2.

2. In TIG process it is ER 80 S-D2

Sridhar.



From: Pawan Pal <pawan...@gmail.com>
To: Materials & Welding <materials-welding@googlegroups.com>
Sent: Saturday, 12 November 2016 3:03 PM
Subject: [MW:25667] Suitable electrodes for joining AISI 4130
Dear Sir,
Thank you for your time to read my question.
 
I want to know which welding electrode is suitable for welding these base metals together  grade AISI 4130 with AISI 4130.
 

 

 
Thanks
 
PAWAN PAL

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/280940935.2724416.1478968951310%40mail.yahoo.com.

For more options, visit https://groups.google.com/d/optout.
--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40Ba8GhrvwT4WAMT%3DBr6064GbEQcUtMWJ2k44sfq7HQP9A%40mail.gmail.com.

c sridhar

unread,
Nov 14, 2016, 10:33:47 PM11/14/16
to material...@googlegroups.com
ER 70S-D2 is TIG is TIG filler wire and used when  4130 is joined joined with a mild steel . 

4130 being a alloy product with Cr & Mo and when welded with same metal, mechanical 
and chemical properties to be considered.



From: Kannayeram Gnanapandithan <kgpan...@gmail.com>
To: materials-welding <material...@googlegroups.com>
Sent: Monday, 14 November 2016 10:34 AM
Subject: Re: [MW:25687] Suitable electrodes for joining AISI 4130

ER 70S-A1

For more options, visit https://groups.google.com/d/op tout.
--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
To post to this group, send email to materials-welding@ googlegroups.com.

For more options, visit https://groups.google.com/d/ optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eN0qssdkF5OU367Dw9iPC%3DPTTbMkd%3Dr%2BewJE9q_L_mG_g%40mail.gmail.com.
Reply all
Reply to author
Forward
0 new messages