E-7018-1 is better then E7018

525 views
Skip to first unread message

Ghulam Mustafa

unread,
Sep 2, 2020, 2:00:08 AM9/2/20
to Materials & Welding
Dear All,
Hope you are fine.
i want discuss that i was gone yesterday for inspection in other company as a third party, i checked WPS for welding inspection, during inspection i observed that welder used E7018-1 Electrode instead of E7018 on structure. structure material A572 Grade-B and A-36. E7018-1 can problem or not?
can any one tell me about this problem.

yomna Ahmed

unread,
Sep 2, 2020, 2:14:19 AM9/2/20
to material...@googlegroups.com
No proplems

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b55e87f5-633e-477c-b7ad-be9aa33fcd52n%40googlegroups.com.

Mohamed Elsayed

unread,
Sep 2, 2020, 2:45:08 AM9/2/20
to material...@googlegroups.com
The difference between E 7018 and 7018-1 is the impact test temperature, so 7018-1 is better than 7018

Sourav Bohrays

unread,
Sep 2, 2020, 2:45:08 AM9/2/20
to material...@googlegroups.com
only difference is impact test temprature.

Chandan Singh

unread,
Sep 2, 2020, 2:45:09 AM9/2/20
to material...@googlegroups.com
Dear ,

There is no problem, basically E7018-1 electrode used for Impact Value.




--


https://materials-welding.blogspot.com/


https://www.linkedin.com/groups/122787


---


You received this message because you are subscribed to the Google Groups "Materials & Welding" group.


To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.


To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b55e87f5-633e-477c-b7ad-be9aa33fcd52n%40googlegroups.com.




--
Regards
CHANDAN SINGH
Sterling & Wilson 
+919981575817
+917379619175




--
Regards
CHANDAN SINGH
Sterling & Wilson 
+919981575817
+917379619175


George Dilintas

unread,
Sep 2, 2020, 8:20:24 AM9/2/20
to material...@googlegroups.com
Better performance in low temperature. Same A and F-no

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b55e87f5-633e-477c-b7ad-be9aa33fcd52n%40googlegroups.com.


--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

HENNING John

unread,
Sep 2, 2020, 11:49:31 AM9/2/20
to material...@googlegroups.com

Consider it to be a premium subset of the E7018.  Basically same properties but with chemistry optimized to achieve low temperature impact properties.  It is generally acceptable to use E7018-1 in lieu of E7018 unless customer has specific requirements regarding qualification. 

 

Code is fun. Enjoy.

DISCLAIMER This e-mail and any attachments thereto may contain information which is confidential and/or protected by intellectual property rights and are intended for the sole use of the recipient(s)named above. Any use of the information contained herein (including, but not limited to, total or partial reproduction, communication or distribution in any form) by persons other than the designated recipient(s) is prohibited. If you have received this e-mail in error, please notify the sender either by telephone or by e-mail and delete the material from any computer.
General Data Protection Regulation (GDPR)
We respect and protect your privacy to provide you with our services. Please read https://www.hamon.com/customer-data-protection-notice (Customer) and https://www.hamon.com/seller-data-protection-notice (Supplier) how we process your personal data.

Thank you for your cooperation.
______________________________________________________________________

pgos...@rogers.com

unread,
Sep 2, 2020, 4:06:37 PM9/2/20
to material...@googlegroups.com

Hi Ghulam,

E 7018-1  electrodes contains more Mn than E-7018 electrode, at the same strength(UTS) level, 70 Ksi. The advantage is better impact . Typically E-7018-1 are designed for impact up to -46 Deg c , while the same for E-7018 is up to -29 Deg C.

In order to avoid duplicity or redundant work nowadays  it’s very commons for electrode manufacturers to classify same welding electrode as E-7018-1/E-7018, which is called dual certification.

Please look at the highlighted text from, SFA 5.1 , Sec-II, Pt-C, on E-7018-1 welding electrodes.

As the mechanical and other properties of the deposited are not changed, a change from E-7018 to E-7018-1 , will not cause any harm the welds . However if should be addressed in WPS or regularized through an NCR.

 

Thanks

 

Pradip Goswami, P.Eng, IWE

Consultant-Welding-Metallurgical Engineering

 

Cell & Whatsapp-905-9793232.

Personal:pgos...@rogers.com

 

 

--

https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b55e87f5-633e-477c-b7ad-be9aa33fcd52n%40googlegroups.com.




AVG logo

This email has been checked for viruses by AVG antivirus software.
www.avg.com


image003.jpg

Kannayeram Gnanapandithan

unread,
Sep 2, 2020, 11:36:29 PM9/2/20
to materials-welding
When subjected to SR, 7018-1 gives better mechanical value compared to 7018 due to more manganese in -1. Better ductility , cost is more

james gerald

unread,
Sep 3, 2020, 12:05:43 AM9/3/20
to material...@googlegroups.com
Hi Mr. Goswami,

Please can you throw some Light on the Manganese content of E7018 & E 7018-1 as AWS 5.1 restricts Manganese to 1.6% and what will happen if increased beyond this range.

Thanks & Regards

J.Gerald Jayakumar




Guru. Thilakar

unread,
Sep 5, 2020, 7:02:42 AM9/5/20
to material...@googlegroups.com
E7018-1 is good weld ability for above 32 thickness, last month in structural I welded E7018 for 32mm thk web with 32mm thk flange IS2062 all the fillet joint CRACKED immediately. So after that we used E7018-1 no crack observed.

Regards, 
Gurugopal.P.G 

Ghulam Mustafa

unread,
Sep 8, 2020, 1:31:49 AM9/8/20
to material...@googlegroups.com
Thanks to all of you for solving these problems.