SS 304 to SS 321 welding

974 views
Skip to first unread message

hrish...@gmail.com

unread,
Nov 25, 2010, 8:15:58 AM11/25/10
to Materials Welding
1.Pl advise if SS 304 to SS 321 piping welding is possible? If so what is the consumable to be used
2. Is welding of SS 321 possible with E 308 consumable provided one has an approved WPS/PQR?

Thanks
Hrishi
Sent on my BlackBerry® from Vodafone

Ramprasad Chari

unread,
Nov 26, 2010, 2:43:23 AM11/26/10
to material...@googlegroups.com
You need to weld with FW ER347 or Electrode E347-15/16
Regards
Aarpee


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Majdi N Elyyan

unread,
Nov 26, 2010, 3:15:14 PM11/26/10
to material...@googlegroups.com

Dear All

 

Just to share the attached article with all

 

Regards

Majdi Elyyan

Failure analysis of a welded outlet manifold pipe in a primary steam reformer by improper selection of materials.pdf

Duraimurugan Subramanian

unread,
Nov 27, 2010, 12:17:42 AM11/27/10
to material...@googlegroups.com
Dear Hrishi
 
 
you need to weld with ER308L / ER308L-15 Electrodes.
 
 
Regards
 
Durai Murugan
QC Welding Inspector


From: "hrish...@gmail.com" <hrish...@gmail.com>
To: Materials Welding <material...@googlegroups.com>
Sent: Thu, November 25, 2010 4:15:58 PM
Subject: [MW:8385] SS 304 to SS 321 welding
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com

Yogesh kumar

unread,
Nov 27, 2010, 2:59:17 AM11/27/10
to material...@googlegroups.com
You may go with ER309MoL also to weld 321/304 with due consideration of heat input.

To unsubscribe from this group, send email to materials-weld...@googlegroups.com

Mayur Purwant

unread,
Nov 27, 2010, 10:10:13 AM11/27/10
to material...@googlegroups.com
pl advise,
 
I am Facing problem in SS304L welding,
 
The job requirement is,
Welding of SS304  12mm thk plates with SS308L filler wire i.e. TIG120 (GTAW only) in 3G position and the RT of the joint is as per sec III.
 
When I did welding, I found Clusters and Porosity in RT film, I did trials for the same on 200 mm length coupon with same thk base material and it found OK in RT.
 
Again I decided to weld job with puting same parameters as per mock up, But surprisingly in RT film again the same problem was observed i.e. clusters and porosity.
 
Please advise me hoe to minimise or reduce this problem. 
 
 
Regards,
Mayur

kannayeram gnanapandithan

unread,
Nov 28, 2010, 7:36:03 AM11/28/10
to material...@googlegroups.com
308L is ok for dissimilar weld of this combination
genearally major alloying elements composition is same for both except 321 is stabilized steel,
kgp

On Thu, Nov 25, 2010 at 6:45 PM, <hrish...@gmail.com> wrote:

Yogesh kumar

unread,
Nov 28, 2010, 7:45:48 AM11/28/10
to material...@googlegroups.com
  • ensure proper purging of the weld joint
  • the quality of argon gas in GT AW
  • proper shielding of job


regards