filler wire identification required.

已查看 81 次
跳至第一个未读帖子

rahmat khan

未读,
2021年12月27日 05:49:402021/12/27
收件人 Materials & Welding
Dear All,

Please help me in this to find the exact filler wire to be used for dissimilar material:

1)  SB 424 Incoloy 825  (P45 material)       to    2)  A 105 (Carbon steel P1 material)

please help me in this to find the exact selection.

Kannayeram Gnanapandithan

未读,
2021年12月27日 06:20:022021/12/27
收件人 materials-welding
NiCrMo3

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/decea44d-1b3b-4c7d-aaf1-7462bad96cd4n%40googlegroups.com.

rahmat khan

未读,
2021年12月28日 22:35:302021/12/28
收件人 Materials & Welding
Thanks for the answer.

i want to know on which factors you have decided to go with ER-NiCrMo-3, I mean there can be some middle-range filler selected.

Kannayeram Gnanapandithan

未读,
2021年12月29日 02:33:402021/12/29
收件人 materials-welding
To have better ductility and tolerance of dilution by iron, matching with base metal.

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

james gerald

未读,
2021年12月29日 02:54:202021/12/29
收件人 material...@googlegroups.com
Refer attached

Thanks & Regards

J.Gerald Jayakumar