Oxidation during welding of SA213 gr T22

144 views
Skip to first unread message

hvala...@gmail.com

unread,
Oct 5, 2023, 10:00:39 AM10/5/23
to Materials & Welding
Dear experts,

We are facing problems with welding of SA 213 Gr T22 superheater tubes of thickness 2.9mm.

Generally, back purging with inert gas in GTAW is not necessary for P22 as Cr is less than 3%. However, during welding without use of back purging, Oxide formation is happening. The construction of the equipment is such that, purging is very difficult to achieve.

Kindly Guide us to eliminate the oxidation of root.

Thanking you,
Alpesh


tamilneethi thennavan

unread,
Oct 6, 2023, 4:52:32 AM10/6/23
to material...@googlegroups.com
Dear Mr.Alpesh,

As your statement is wrong.as per API RP 582 Shielding and Purging Gases Clause 7.3 Back purging is required for the GTAW and GMAW processes for welding materials having a nominal chromium
content greater than 2-1/4 %, 

Capture.PNG

So you better try back purging....... 

Thanks.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/e2e41e16-2ea6-419a-8e20-9121f424edd5n%40googlegroups.com.


--
Regards,

Tamil Neethi.T


                 

Vishwas Keskar

unread,
Oct 6, 2023, 8:34:33 AM10/6/23
to material...@googlegroups.com
For Gr 22 purging is not required
You can do following 
Use lower dis filler wire dia 1.6 
Use injection purging. Method means : inject. Gas from groove root gap
This shall ensure better quality of Welding 

Vishwas -IWE
International Welding Engineer


Sent from my iPhone

On 06-Oct-2023, at 2:22 PM, tamilneethi thennavan <tamilne...@gmail.com> wrote:


Dear Mr.Alpesh,

As your statement is wrong.as per API RP 582 Shielding and Purging Gases Clause 7.3 Back purging is required for the GTAW and GMAW processes for welding materials having a nominal chromium
content greater than 2-1/4 %, 

Kannayeram Gnanapandithan

unread,
Oct 6, 2023, 8:34:33 AM10/6/23
to materials-welding

Prakash Hegde

unread,
Oct 9, 2023, 2:54:58 AM10/9/23
to material...@googlegroups.com
Hi
My experience with LAS welding by GTAW
Filler wire with above 1.4 Cr say EB2
It is better to use Argon purging for FPW for GTAW to avoid Oxidation of weld for root

Regards
Hegde

Vishwas Keskar

unread,
Oct 10, 2023, 3:42:08 AM10/10/23
to material...@googlegroups.com
P22/T22 is 
2.25 Cr , 1 Mo 


Sent from my iPhone

On 09-Oct-2023, at 12:24 PM, 'Prakash Hegde' via Materials & Welding <material...@googlegroups.com> wrote:

Hi

Kalpesh Mehta

unread,
Oct 16, 2023, 3:22:24 AM10/16/23
to material...@googlegroups.com
Dear all,
Can anyone share underwater training material and WPS /PQR ? 
Regards 

Ramon Briceno

unread,
Oct 24, 2023, 9:12:36 AM10/24/23
to material...@googlegroups.com
Please continue with the back purge. GTAW and GMAW require it.
Also, welding of T22 demand the major care,  cleaning and free oxidation.

Regards,
Ramon Briceno
Metallurgical Engineer.



From: material...@googlegroups.com <material...@googlegroups.com> on behalf of hvala...@gmail.com <hvala...@gmail.com>
Sent: Tuesday, October 3, 2023 3:33:15 AM
To: Materials & Welding <material...@googlegroups.com>
Subject: [MW:34562] Oxidation during welding of SA213 gr T22
 
Reply all
Reply to author
Forward
0 new messages