The current circumstances is ,
Vessel is SS316 and I am welding a SS316 4mm plate on the CS flange as a cladding.
I want to know if I weld the SS316 Cladding plate on CS Flange with SS309. is it any problem with their composition?
Second is that SS309 is compatible with SS316 if I totally weld with SS309 Electrode.

Regards,
Mailsuite Sent with Mailsuite  ·  Unsubscribe
06/05/24, 12:42:33 PM

Amol Betkar

unread,
Jun 5, 2024, 4:12:23 AMJun 5
to material...@googlegroups.com

Dear Mashood,

When welding stainless steel to carbon steel or when dealing with different grades of stainless steel, the choice of filler material is critical to ensure the integrity and performance of the weld.

Welding SS316 to a CS Flange with SS309

  1. Using SS309 as a filler for welding SS316 to CS:

    • Composition and Compatibility:
      • SS309: This grade is often used as a filler metal for welding dissimilar steels, including stainless steels to carbon steels. SS309 contains higher chromium and nickel content than SS316, which helps in accommodating the differences in thermal expansion and enhancing corrosion resistance at the weld interface.
      • SS316 and Carbon Steel (CS): Carbon steel (CS) has a different composition and thermal properties compared to SS316. SS316 is an austenitic stainless steel with molybdenum added for improved corrosion resistance.
      • SS309 filler metal is designed to bridge the differences in composition between SS316 and CS. It can handle the dilution from the carbon steel and provide a good quality weld with adequate corrosion resistance and mechanical properties.
    • Potential Issues: Using SS309 should not present significant problems in terms of composition. The SS309 filler is designed to manage the differences in expansion rates and chemical composition between stainless and carbon steel, making it a suitable choice for cladding SS316 on a CS flange.
  2. Using SS309 for welding SS316 completely:

    • Compatibility of SS309 and SS316:
      • SS309 is generally compatible with SS316, though it is typically used for welding dissimilar metals.
      • Mechanical Properties: SS309 will have slightly different mechanical properties and corrosion resistance compared to SS316. While SS309 is more oxidation-resistant at higher temperatures, SS316 offers better overall corrosion resistance due to its higher molybdenum content.
      • Weld Characteristics: When welding SS316 with SS309, the resulting weld may have different properties than a weld made entirely with a filler matching SS316. This could include slight differences in corrosion resistance and mechanical properties in the weld zone.
    • Potential Issues: While there is generally no problem using SS309 to weld SS316, the resulting weld might not fully match the performance characteristics of the base SS316 material, particularly in environments where SS316's specific properties are crucial (such as resistance to certain types of corrosion).

Recommendations:

  • For Cladding Application: Using SS309 to weld the SS316 cladding plate to the CS flange is appropriate and should not cause significant issues in terms of composition or weld quality.
  • For Welding SS316 Components: If the application demands the specific properties of SS316, it is preferable to use a filler that matches SS316 to ensure consistent properties throughout the weld. However, if slight differences in properties are acceptable, SS309 can be used without major concerns.

In summary, SS309 is a suitable filler material for welding SS316 to a CS flange and is generally compatible with SS316 for welding purposes, though attention should be given to the specific application requirements.


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAD3cn5hS2LbPHDo%3DciN_dsPUK9X-97b33KRO80PYso_cLw6rjw%40mail.gmail.com.


--
Best regards,

Amol K.B
B.E(Mech), CSWIP 3.2.2, NACE CIP 1 & ASNT LII(4M)

sridhar cn

unread,
Jun 6, 2024, 5:52:07 AMJun 6
to material...@googlegroups.com
Since you are using SS316 to CS, it will be appropriate to use E309Mo or ER309Mo in place of E309 
as SS 316 contains Mo besides Cr & Ni.
C Sridhar

Kannayeram Gnanapandithan

unread,
Jun 10, 2024, 2:34:28 AMJun 10
to material...@googlegroups.com
It is better to use 309MoL

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--

Parminder Singh

unread,
Jun 10, 2024, 2:59:00 AMJun 10
to material...@googlegroups.com
Dear, 

Use 309Mo for better results 

On Wed, Jun 5, 2024 at 1:21 PM Mashood Khan <mas...@epic.com.pk> wrote:
--

Mohd Siraj

unread,
Jun 12, 2024, 11:29:18 AMJun 12
to Materials & Welding
dear,

what if you could do weld overlay  (similar to buildup with same chemistry) ?, welding plate on flage may be tricky to match curvature? what you say?