REGARDING ISSUE IN MONEL 400 TUBE TO TUBESHEET JOINT WELDING

97 views
Skip to first unread message

Saurabh Joshi

unread,
Jul 4, 2023, 12:37:22 AM7/4/23
to Materials & Welding
Dear All, 


       We are facing cracking  of tube ends , dis-bonding between tube base material and filler material during welding in Monel 400 Tube to Tubesheet Joints. Refer attached photographs.
Tube MOC: SB-163 UNS-N04400; 25.0 mm OD x 2.0 mm thk
Tube sheet MOC: SA-336M Gr F304L + SB-127 UNS-N04400 (48 + 10 mm thick clad by Explosion Bonding)
Welding: ERNiCu-7 GTAW filler size 2.0mm  with Argon shielding gas.


Kindly share the reason for such cracking, disbonding  and Suggest Corrective and preventive actions regarding this issue.

Thanks in Advance.

PHOTO-2023-07-03-16-23-10 (1).jpg
PHOTO-2023-07-03-16-22-47.jpg
PHOTO-2023-07-03-16-23-10.jpg

Kannayeram Gnanapandithan

unread,
Jul 4, 2023, 1:39:44 AM7/4/23
to material...@googlegroups.com
Welder skill is very important, Too much current,
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/70d8c114-8503-4ad0-b5db-22db6d57871en%40googlegroups.com.

Prakash Hegde

unread,
Jul 4, 2023, 2:15:48 AM7/4/23
to material...@googlegroups.com
Hi
Monel T/Tsht jt welding needs practice to welder for manovering the arc and welding direction
7 o clock to 2 o'clock 6 o clock to 10 o clock  3  to to 11 and.9 to1
As monel weld pool is sluggish hence Groove angle should be shallow with 35 to 40 degree
Increase the current with arc direction should be directed toward tube sht side and not on tube
Try with 1.6dia wire
Try and practice
Regards

Parminder Singh

unread,
Jul 5, 2023, 5:11:44 AM7/5/23
to material...@googlegroups.com
control heat input
welder skill of controlling monel weld pool