Hello,

I have individual qualified welders per BPVC Section-IX-2015, as per following detail:

1. P1,G1 TO P1,G1

2. P8,G1 TO P8,G1

Can I use the same welder for welding of following?

1. P1,G1  TO P8,G1 

Thanking You,

Surendra
Bhilwara, Rajastha(Ind)


Ramesh

unread,
Nov 12, 2018, 12:31:12 AM11/12/18
to material...@googlegroups.com

Hi

 

Pl refer QW-350 for the essential variable for Welder.

 

QW-351 GENERAL “ A welder shall be requalified whenever a change is made in one or more of the essential variables listed for each welding process.”

 

WPQ is not only depend on P numbers, there are other variables are also to be considered.    

Pl check your essential variable against your welding process.

 

Example For SMAW,

 

Change in base metal  P no is essential variable, i.e. QW- 403.18


image.png

Thanks and Regards


Rameshkannan Devaraj

"What you have learned is a mere handful; What you haven't learned is the size of the world – Avvaiyar"



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Souravbohray

unread,
Nov 12, 2018, 12:48:05 AM11/12/18
to Materials & Welding
Can't use because change in P no Nd u dnt hv qualified for p8 to p1. You have only p1 to p1 and p8 to p8.
you have qualified cs to cs and as to ss.
But u dnt hv qualified ms to ss .it's different u cnt use .if I m wrong correct me.

Surendra

unread,
Nov 12, 2018, 12:54:48 AM11/12/18
to material...@googlegroups.com
U r correct!

rajesh kaswala

unread,
Nov 12, 2018, 5:20:53 AM11/12/18
to material...@googlegroups.com
refer this

QW-423 Alternate Base Materials for Welder
Qualification

image.png



regard
rajesh

munee...@gmail.com

unread,
Nov 12, 2018, 5:20:54 AM11/12/18
to materials-welding
I have individual qualified welders per BPVC Section-IX-2015, as per following detail:
1. P1,G1 TO P1,G1
2. P8,G1 TO P8,G1
Can I use the same welder for welding of following?
1. P1,G1  TO P8,G1 

REPLY:
Read QW-350 will describe you the most common factors affecting the essential variables of process like dimater, thickness, t weld depostions, main factors in your case listed as per below,
1) Approved procedure (WPS) for your dissimilar.
2) Should not be change in F-no (WPS vs WPQ-Performance) same F.
3) Should not omit inert gas backing on the job.
4) Lastly clarity on P1,G1 TO P1,G1 and P8,G1 TO P8,G1 qualified welder to P1,G1  TO P8,G1 disimilar, for this scenario both welders can weld as this scenario will not have omit in backing gas , with same F nos on job and as per QW-423 table.
5) Refer QW-350, 408.8, QW-423 and QW-433
Concluding that if your production ensured with all common and main factorts above, then yes you can.
Regards,
Mohamed Muneeb Mahaboob
CSWIP 3.2-89247/2
AWS-CWI (2007)
ASNT-NDT-L2-RTFI-RT-UT-MT-PT.
SA SAP#:70021650 JAPID, QCS & QCI.
+91-636-955-7189 & +91-801-521-6854.
From: Surendra
Date: 2018-11-12 13:22
Subject: [MW:28617] RE: 28616] Welder qualification
U r correct!
 
-----Original Message-----
From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Souravbohray
Sent: 12 November 2018 11:17
To: Materials & Welding
Subject: [MW:28616] Welder qualification
 
Can't use because change in P no Nd u dnt hv qualified for p8 to p1. You have only p1 to p1 and p8 to p8.
you have qualified cs to cs and as to ss.
But u dnt hv qualified ms to ss .it's different u cnt use .if I m wrong correct me.
 
--
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
 
--
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
Date: 2018-11-12 12:46
Subject: [MW:28616] Welder qualification
Can't use because change in P no Nd u dnt hv qualified for p8 to p1. You have only p1 to p1 and p8 to p8.
you have qualified cs to cs and as to ss.
But u dnt hv qualified ms to ss .it's different u cnt use .if I m wrong correct me.
 
Catch25CE(11-12-16-19-35)(1).jpg
image(11-12-14-5(11-12-16-19-35)(1).png

Aslam Khan

unread,
Nov 12, 2018, 8:03:58 AM11/12/18
to material...@googlegroups.com
No, as P. No. is essential variable, you have to qualify WPQ with new PQR.

Surendra

unread,
Nov 12, 2018, 8:03:58 AM11/12/18
to material...@googlegroups.com

Thanks Mr Mahaboob,

 

Now I can use same qualification for dissimilar material as described below.

 

Regards,

 

Surendra

image001.jpg
image002.png

George Dilintas

unread,
Nov 22, 2018, 10:43:49 PM11/22/18
to material...@googlegroups.com
You cannot 

munee...@gmail.com

unread,
Nov 22, 2018, 11:25:48 PM11/22/18
to materials-welding
Greetings George,

It would be intresting if we know why it is not possible for this below case? with references, so that we can learn / adopt, your point of view, if it is acceptable.

Thanks.

Regards,
Mohamed Muneeb Mahaboob
CSWIP 3.2-89247/2 
ASNT-NDT-L2-RTFI-RT-UT-MT-PT.
SAP#:70021650 APs:JAPID, QCS & QCI.
munee...@gmail.com +91-636-955-7189

(6:59) He has the keys to the realm that lies beyond the reach of human perception; none knows them but He. And He knows what is on the land and in the sea; there is not a leaf which falls that He does not know about and there is not a grain in the darkness of the earth or anything green or dry which has not been recorded in a Clear Book.

 
Date: 2018-11-23 00:35

José Juan Jiménez Alejandro

unread,
Nov 23, 2018, 9:28:46 PM11/23/18
to material...@googlegroups.com
This topic seems quite interesting and I see divided opinions, I allow myself to give my opinion and if it is incorrect I hope that someone with more experience will give us more light and knowledge on this important topic.
Attached image of a part of a Welder Qualification, this was used for an ASME Audit, in other words it was reviewed by the ASME Authorized Inspector; two points:
1.- ASME IX works very differently than D1.1 does.
2.- In the column with red box: Range Qualified cross with Metal Base, there is a list of Numbers P (1 THROUGH 15F; 34 AND 41 THROUGH 49), I understand that the welder in this case was qualified for P1 with P1 but that has the ability and qualification to weld all P1 THROUGH P15F steels; P34 AND P41 THROUGH P49 and the combinations between these materials. It should be mentioned that this is suggested to the F-number, qualified position, thicknesses and diameters. in fact in an API course I heard that under ASME IX only three coupons are needed to qualify a welder in all materials, this if you do not take into account: F number, position, thicknesses and diameters. I will thank you infinitely for your contributions.

Libre de virus. www.avast.com

Ing. José Juan Jiménez Alejandro

ASME Independent Consultant 

and Technical Manager SSI-TPI

Cel. +52 812 352 4606

Skype: jjjimeneza

Twitter: @jjjimeneza




Libre de virus. www.avast.com
WPS.jpg

Karthik

unread,
Nov 23, 2018, 9:28:46 PM11/23/18
to material...@googlegroups.com
Hi,
As per QW423, you can weld if all other essential variables are met as per QW350.

Inline image


Thanks& Regards,

 

(Karthik)

Karthikeyan.S

QA/QC Manager
Agon Pacific Co.,Ltd.
M: +66-655-174-397, +66-892-512-282

E-mail : karthi...@yahoo.com



munee...@gmail.com

unread,
Nov 24, 2018, 7:20:12 AM11/24/18
to materials-welding
Agreed, P1 qualified can go through all materials as mentioned by QW-423.1 , hence below scenario becomes acceptable as P1,G1 TO P1,G1 and P8,G1 TO P8,G1 qualified welder to P1,G1  TO P8,G1 disimilar, both welders can weld as this scenario will not have omit in backing gas , with same F nos on job and as per QW-423 table.

But still any members can enlight their vision for acceptabnce / non acceptance with references.

Thanks.


Regards,
Mohamed Muneeb Mahaboob
CSWIP 3.2-89247/2 
ASNT-NDT-L2-RTFI-RT-UT-MT-PT.
SAP#:70021650 APs:JAPID, QCS & QCI.
munee...@gmail.com +91-636-955-7189

(6:59) He has the keys to the realm that lies beyond the reach of human perception; none knows them but He. And He knows what is on the land and in the sea; there is not a leaf which falls that He does not know about and there is not a grain in the darkness of the earth or anything green or dry which has not been recorded in a Clear Book.

Date: 2018-11-24 03:12

DINESH SHARMA

unread,
Nov 24, 2018, 7:20:12 AM11/24/18
to material...@googlegroups.com
Yes I agree
You can use that welder because welder nor qualified with other than P1 and 8

Thanks
Dinesh Sharma



From: George Dilintas <dili...@gmail.com>
Sent: Fri, 23 Nov 2018 09:13:48 GMT+0530
To: material...@googlegroups.com
Subject: Re: [MW:28660] Welder qualification

You cannot 

Στις Κυρ, 11 Νοε 2018, 04:19 ο χρήστης Surendra <skchor...@gmail.com> έγραψε:
Hello,

I have individual qualified welders per BPVC Section-IX-2015, as per following detail:

1. P1,G1 TO P1,G1

2. P8,G1 TO P8,G1

Can I use the same welder for welding of following?

1. P1,G1  TO P8,G1 

Thanking You,

Surendra
Bhilwara, Rajastha(Ind)


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

For more options, visit https://groups.google.com/d/optout.
Reply all
Reply to author
Forward
0 new messages