DEAR EXPERTS

My question is about RT rules according to asme sec VIII
is it possible to use ut ( according to code case 2235-9 )  instead of rt in Inspection of joints efficiency = 1.00 ? 
or we can use it just when the construction does not permit interpretable radiographs in accordance with Code requirements ?
and my second question:
Is it possible using of division 2 roles for inspection of weld joints when general design and fabrication specification is according to division 1?

Best regards.

-----------------------------------------------------
according to division 1

1:
 Table uw-12:
full rt is required for joint efficiency = 1.00
2:
uw-11
(8) ultrasonic examination in accordance with UW-53 may be substituted for radiography for the final closure seam of a pressure vessel if the construction of the vessel does not permit interpretable radiographs in accordance with Code requirements. The absence of suitable radiographic equipment shall not be justification for such substitution.
3:
UW-51- (4)
 As an alternative to the radiographic examination requirements above, all welds in material 6 mm and greater in thickness may be examined using the ultrasonic method per the requirements of 7.5.5 of Section VIII, Division 2.

division 2:
and according to division 2 Table 7.2 There is the possibility of using both UT or RT for joint efficiency = 1.00
-------------------------------------------

george....@gr.bureauveritas.com

unread,
Dec 12, 2015, 12:04:50 AM12/12/15
to Materials & Welding
When thickness is not lower than 6 mm you may use UT for any joint but in accordance with Div. 2. If thickness us lower than 6 mm you can use UT only for the situation described in UW11(8)

Sent from my BlackBerry 10 smartphone.
From: Mehdi Vafakhah
Sent: Παρασκευή, 11 Δεκεμβρίου 2015 - 12:35
To: Materials & Welding
Subject: [MW:23964] ASME SECVIII RT RULES

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/d5024827-f951-4c55-883e-a040f4ab7b22%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Jay Poojary

unread,
Dec 12, 2015, 11:43:09 AM12/12/15
to material...@googlegroups.com
Also for the acceptance criteria see table 7.5, which is very difficult to produced on demo piece. Better to go for RT for less thickness.