Shielding gas for GMAW pulsed welding-Carbon Steel

76 views
Skip to first unread message

Aby Jose

unread,
Mar 21, 2017, 6:57:30 AM3/21/17
to material...@googlegroups.com
Dear all,

What shielding gas should be used for the pulsed GMAW welding of carbon steel? When trying with 80%Ar+20%CO2 mixture I am getting a lot of spatters. The welding used is Automatic welding with Robotic machine.
Any recommendations???

Regards,
Aby

Kannayeram Gnanapandithan

unread,
Mar 21, 2017, 8:03:01 AM3/21/17
to materials-welding
what are welding parameters

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACdTRdyc8NMn6LBHHHTeYFxP_Ani0cnWDw0j5qEJSyRyfoOe4Q%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

PGoswami

unread,
Mar 21, 2017, 8:33:58 AM3/21/17
to material...@googlegroups.com, pgos...@quickclic.net

Hi Aby,

 

More enriched version of mixed gases, e.g. 90Ar+10 O2 or other Ar enriched blends may help. Look at this guide ,which has few  good recommendations about shielding gases.

 

Thanks.

 

P.Goswami,P.Eng,IWE.

 

https://www.lincolnelectric.com/assets/global/products/consumable_miggmawwires-superarc-superarcl-56/c4200.pdf

--

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.




AVG logo

This email has been checked for viruses by AVG antivirus software.
www.avg.com


Prasad Rao

unread,
Mar 21, 2017, 10:46:43 PM3/21/17
to material...@googlegroups.com
Try for 98% argon and 2% co2

On Tue, Mar 21, 2017 at 12:56 PM, Aby Jose <abyc...@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (abyc...@gmail.com) Add cleanup rule | More info

Dear all,

What shielding gas should be used for the pulsed GMAW welding of carbon steel? When trying with 80%Ar+20%CO2 mixture I am getting a lot of spatters. The welding used is Automatic welding with Robotic machine.
Any recommendations???

Regards,
Aby

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

Kannayeram Gnanapandithan

unread,
Mar 21, 2017, 11:35:55 PM3/21/17
to materials-welding
As argon increase, %of penetration will come down and may get into porosity .  Try with 85+15 with current of >250amps. spatter is inevitable in this process, u can reduce by another option with GMAW-P. If u work in Spray mode, spatter stiking into base metal will be less due to its sizes

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Tue, Mar 21, 2017 at 7:12 PM, Prasad Rao <prasa...@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (prasa...@gmail.com) Add cleanup rule | More info

Diganta Sarma

unread,
Mar 21, 2017, 11:47:37 PM3/21/17
to material...@googlegroups.com
A 20% carbon di oxide mix in a 80% argon usually works best in spray transfer mode in w position so you would need to ensure that you aren't using short circuiting mode which is resulting in large amount of spatters. In case you're welding thin sheets or doing out of position welding you may have to consider changing the gas mixture 

Trust this helps

Sent from my iPhone
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEML-XRowcwexs%3DZz4xzozQA7Q6p6XcbJr1YNpG98vBsr-o90w%40mail.gmail.com.

Perumal Govindan

unread,
Mar 21, 2017, 11:59:51 PM3/21/17
to material...@googlegroups.com

Hi Jose,
Please let me know the AWS classification of filler wire and brand used or please follow the manufacturer recommendation for choosing the shielding gas or refer the filler wire data sheet.

Regards
P Govindan

Aby Jose

unread,
Mar 22, 2017, 2:37:49 AM3/22/17
to material...@googlegroups.com
Hi Perumal,

I am using ER 70S6 and the manufacturer is Bohler.

Regards,
Aby

Aby Jose

unread,
Mar 22, 2017, 2:37:55 AM3/22/17
to material...@googlegroups.com
Dear Mr Pandithan,

In the machine I have selected the pulse mode itself. (GMAW-P). The position I am using is IG(rotating ) . As I am using the synergy mode in the machine the current and voltage is getting selected automatically when I am giving the wire feed speed. I am using the wire feed speed of 9.5 m/min, the voltage coming is in range 25V -28V and current in range 215 to 230. How to ensure I am not using the short circuiting mode?? I am using this process for pipe welding which includes both high and low thickness.

Regards,
Aby

Kannayeram Gnanapandithan

unread,
Mar 22, 2017, 9:50:10 AM3/22/17
to materials-welding
Voltage anything less than 21v goes to short circuit, but in ur case Voltage is ok, but increase the current to minimum 250amps, Do not put in Synergy mode and set the Current as required.

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Wed, Mar 22, 2017 at 10:06 AM, Aby Jose <abyc...@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (abyc...@gmail.com) Add cleanup rule | More info

Dear Mr Pandithan,

In the machine I have selected the pulse mode itself. (GMAW-P). The position I am using is IG(rotating ) . As I am using the synergy mode in the machine the current and voltage is getting selected automatically when I am giving the wire feed speed. I am using the wire feed speed of 9.5 m/min, the voltage coming is in range 25V -28V and current in range 215 to 230. How to ensure I am not using the short circuiting mode?? I am using this process for pipe welding which includes both high and low thickness.

Regards,
Aby
On Wed, Mar 22, 2017 at 9:02 AM, Kannayeram Gnanapandithan <kgpan...@gmail.com> wrote:

For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

Perumal Govindan

unread,
Mar 23, 2017, 6:49:03 AM3/23/17
to material...@googlegroups.com

Hi Jose,

As per data sheet of ER70S-6, Bohler EMK 6, recommended composition of shielding gas is Ar + 15 to 25% of CO2.

Regards
P Govindan

Aby Jose

unread,
Mar 24, 2017, 12:31:38 AM3/24/17
to material...@googlegroups.com
Yeah Mr Perumal. But by using Ar + 20% CO2 I am not able to control the spatter that is the problem.

Regards,
Aby

Aby Jose

unread,
Mar 24, 2017, 12:31:41 AM3/24/17
to material...@googlegroups.com
Dear Pandithan,

Here the wire I am using is of dia 1.2 mm. So is it possible to give the current & voltage of that range in the weld layers? The welding process I am following is Root & hotpass TIG and the balance MIG. 

Regards,
Aby

Kannayeram Gnanapandithan

unread,
Mar 24, 2017, 1:46:10 AM3/24/17
to materials-welding
yes

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Thu, Mar 23, 2017 at 9:42 PM, Aby Jose <abyc...@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (abyc...@gmail.com) Add cleanup rule | More info

Dear Pandithan,

Here the wire I am using is of dia 1.2 mm. So is it possible to give the current & voltage of that range in the weld layers? The welding process I am following is Root & hotpass TIG and the balance MIG. 

Regards,
Aby

On Wed, Mar 22, 2017 at 3:36 PM, Kannayeram Gnanapandithan <kgpan...@gmail.com> wrote:

For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.