we have to do qualification wps ,pqr for the below mentioned materials as per ASME section 9.

Test coupon
SA 516 Gr 70 (P-1 G-2) -Thickness 20 mm
with
IS 2062 E 350 C (Unassigned Metal) - Thickness 50 mm
Code - ASME 
Position - 3G
Process - SMAW 
Electrode - E-7018
Impact =  -20C @ 27J

Question
1) what is the minimum & maximum thickness qualified with impact?(code reference).
2) what has to be considered during and after impact results?(comparing with base metals)
3) Whether Thickness "t" weld metal deposit in coupon should be 13 mm or 3 layer minimum in single side to qualify for maximum to be welded ? 

Thanks in advance.Do the needful. 

DEEPAK KASHYAP

unread,
Mar 2, 2024, 12:29:11 AM3/2/24
to material...@googlegroups.com

Dear Mr. Gopalkrishnan,

 

 

As per your query, below are the answers:-

 

  1. The Qualified thickness range of the WPS with impact testing will be Min. 16 to  Max 40 mm (because your weld deposit thickness t will be 20 mm)----refer QW 403.6 and Table QW 451.1
  2. The Group on.  (P1G2 to IS2062 E350C) shall be considered along with above qualified thickness range. ----- refer QW 424.1 and Joule values depends on the Material code/Construction code.
  3. Yes, but it is for welder qualification Not for Procedure. --------- refer Table QW 452.1(b)

 

Thanks

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOp_kKgYrfxS7%2B7LOv5Ow4R%2B1d8WVXgURzsy_NMJZ26nobS9kg%40mail.gmail.com.

Gopalakrishnan G

unread,
Mar 2, 2024, 9:55:54 AM3/2/24
to material...@googlegroups.com
Thanks for your reply.
With the same criteria what will be the qualified Base metal and Thickness qualification for Welder performance qualification (WPQ) and what should be minimum weld deposit to be made if I use 2 welders for the same Test coupon.

DEEPAK KASHYAP

unread,
Mar 4, 2024, 12:26:58 AM3/4/24
to material...@googlegroups.com

Dear Mr. Gopal,

 

In your case, Base material qualification refer QW423.1 , so qualified material range will be P1 to IS2062 E350C .

 

 

For thickness range you have to see the maximum thickness range that will be applicable in your job, and considering the same you have to plan for the minimum weld deposit in your sample which results your welder be applicable for Production welding according to QW-452.1(b)

 

 

 