POST HEATING IN PWHT

146 views
Skip to first unread message

NIKHIL THOMAS JOY

unread,
Oct 26, 2020, 12:42:00 AM10/26/20
to Materials & Welding

Dear sir, Good evening

Sir, kindly please  solve my doubt related to POST HEATING IN PWHT.

1.Where we need to do post heating.

2.If I am doing pwht sudden after welding is there any need of post heating or not.

3.In any code post heating mentioned.

Please give me answer for the above mentioned question.

Chandru Sekar

unread,
Oct 26, 2020, 5:06:35 AM10/26/20
to material...@googlegroups.com

SA 335 grade P9- preheat given 200 degree only as per client requirement then once welding completed , preheat will be increased upto 350 for half an hour.

Rate of heating is same as pwht like 100 degree per hour.

Thanks & Regards
Chan

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/5d07c2d7-f780-459d-8aab-53e92469c23cn%40googlegroups.com.

Vinay Thattey

unread,
Oct 26, 2020, 10:54:01 PM10/26/20
to material...@googlegroups.com, nick.th...@gmail.com
Dear Joy ; In Post weld heat treatment we reheat the weld to generally below critical temperature , golf for given time . It is done to remove / reduce residual stresses and also to obtain favourable microstructure changes  .  For example when there is  risk of  of cracking after  weld , post weld treatment  can be adopted . You need to specify your application , material ,   dimensions etc . Yes post weld treatment is a requirement of code but again details of weld joint, MOC etc are required.



--

Vishwas Keskar

unread,
Oct 27, 2020, 7:45:35 AM10/27/20
to material...@googlegroups.com

1.Where we need to do post heating. -This applicable to High Thickness (@> 50 mm ) Carbon steel  and  @25mm or greater Cr - Mo  (>/= 2.25 Cr steel )steels.

2.If I am doing pwht sudden after welding is there any need of post heating or not. - Then POST HEATING  is not required. But it is practicable ?

3.In any code post heating mentioned.- AWS D10.8-  Cr - Mo steel specifies it 

Please give me answer for the above mentioned questio

--

udaya bhaskar

unread,
Oct 28, 2020, 1:11:39 AM10/28/20
to material...@googlegroups.com
Mr.Nikhil,
Post Heat applicable at,if you done any welding activity after PWHT.


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/5d07c2d7-f780-459d-8aab-53e92469c23cn%40googlegroups.com.


--
With Regards

Udaya bahaskar.D

Kannayeram Gnanapandithan

unread,
Oct 28, 2020, 3:55:17 AM10/28/20
to materials-welding
Post Heat is applicable to bake out Hydrogen before delayed PWHT. When Flux bearing welding process, like FCAW, SMAW, SAW ect  on Higher thickness ( Multiple layers) and Alloy steels to avoid Delayed Crack/ HICC

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


George Dilintas

unread,
Oct 29, 2020, 1:41:27 AM10/29/20
to material...@googlegroups.com
You question is very general.

PWHT depends on the following factors:

Thickness
Material grade
Service requirements (example: lethal service)

For some grades (Pno-15E materials) preheat maintenance is required when PWHT is not done immediately after welding

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/5d07c2d7-f780-459d-8aab-53e92469c23cn%40googlegroups.com.


--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis
Reply all
Reply to author
Forward
0 new messages