ER-70S-2 and ER70S-6

98 views
Skip to first unread message

Chaudhary Zafar Iqbal

unread,
Oct 30, 2022, 11:12:35 PM10/30/22
to material...@googlegroups.com
Respected Member of this Group ,

As per approved wps ER70S-2 required to use .


Any code restrictions to use ER70S-6 instead of ER-70S-2 ?

Any code restriction and reference to change the WPS ?

Waiting for your valuable comments .

Regards,
Zafar 
00966544639978

Muhammad Azeem

unread,
Nov 1, 2022, 5:17:11 AM11/1/22
to material...@googlegroups.com

Hi Zafar,
As per approved WPS you need to follow the same filler wire or electrode, You can switch for welders within the same F number and can use any filler wire.
For WPS strict to utilized as per Actual PQR.

Regards,

Muhammad Azeem Iqbal
Welding Inspector Aramco Approved
053110-8577/0554453626/0590071467




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAP9k9Xfz8xCCsA_t9CeOMw_Z506BBi5sX5wjT8SUuBrS9JrsZQ%40mail.gmail.com.

Vishwas Keskar

unread,
Nov 1, 2022, 11:08:07 PM11/1/22
to material...@googlegroups.com
Approved WPS means you have to use the consumables as per Approved WPS. - ER70S-2 for production welding. 

If you have to write WPS using the same PQR , you can write WPS with ER70S-6 adding note in WPS that Mn content in wire shall  not exceed 1.6 %.
You can resubmit the above WPS  with ER70S6 and get approval for production  welding use.
Pl check read Customer Specification about consumable use.
Vishwas-IWE
International Welding Engineer


Sent from my iPhone

On 31-Oct-2022, at 8:42 AM, Chaudhary Zafar Iqbal <chzai...@gmail.com> wrote:


--

Kannayeram Gnanapandithan

unread,
Nov 1, 2022, 11:08:11 PM11/1/22
to materials-welding
no restrictions  but pl verify the BTC for ER 70S-6 chemistry which Mn, Si shall be within A1 maximum limit. (Mn-1,6, Si-0,8)

srinivas rao

unread,
Nov 2, 2022, 7:07:15 AM11/2/22
to material...@googlegroups.com

code is not restricted  to use these consumables  but WPS shall refer the same consumable which to be used at the time of welding , 
you need to revise this WPS using the same PQR and submit it for client approval before proceeding for welding , u need to mention consumable type which you wants go for 

check client Specification for consumable restrictions against PQR qualified with.

Techinca part :   each consumable has its own advantages but ER70S-6 is better  for strength and impact applications , one  must know that Mn provides better strength and toughness to the weldments. So, any loss of Mn from the weld deposit will actually reduce the strength , more silicon present in ER70S-6 consumable will make a good  weld bead appearance.

Regards, 
Srinivas Rao
Welding Engineer 

Kannayeram Gnanapandithan

unread,
Nov 2, 2022, 7:29:15 AM11/2/22
to materials-welding
unless u verify with BTC or weld metal chemistry ,it is difficult  to decide the A no, because as per sec 2 part C, SFA-5.18, Mn--1.40-1.85 & Si--0.8 -1.15. and as per sec 9, TABLE-QW 442, Mn--1.60max, Si-- 1.00max.  Verify the chemistry and revise the WPS with ER 70-S6