Can anyone suggest suitable filler wires for welding of SS 310 tubes to SS 316L tube sheet? 
Does lack of Mo in ER 310 filler wires makes them unsuitable for the use in hydro-carbon service?
Can we use ER 309L Mo ?

AMOL G

unread,
Aug 11, 2026, 6:47:05 AM (yesterday) Aug 11
to material...@googlegroups.com
ER309L Mo is generally most suitable filler wire.

Thanks,

Amol

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/2393ab33-b01f-4184-b4a7-75381dce4cban%40googlegroups.com.

manish kulkarni

unread,
Aug 11, 2026, 6:47:05 AM (yesterday) Aug 11
to material...@googlegroups.com
Refer API RP 582
--

james gerald

unread,
Aug 11, 2026, 6:58:11 AM (yesterday) Aug 11
to Materials & Welding
What is the operating temperature

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635



--

Ashishranjan - Domech Fabricators Pvt.Ltd.

unread,
6:38 AM (15 hours ago) 6:38 AM
to material...@googlegroups.com
  SS 310S tube + SS 316L tubesheet, GTAW tube-to-tubesheet weld, hydrocarbon service, operating temperature 350°C
  

Regards,

Ashish Ranjan

Go green logo

Save a tree...Please consider your environmental responsibility. Before printing this e-mail message, ask yourself whether you really need a hardcopy.



"Confidentiality Warning: This message and any attachments are intended only for the use of the intended recipient(s), are confidential and may be privileged. If you are not the intended recipient, you are hereby notified that any review, re-transmission, conversion to hard copy, copying, circulation or other use of this message and any attachments is strictly prohibited. If you are not the intended recipient, please notify the sender immediately by return email and delete this message and any attachments from your system.

Virus Warning: Although the company has taken reasonable precautions to ensure no viruses are present in this email. The company cannot accept responsibility for any loss or damage arising from the use of this email or attachment."


Caution: The e-mail below is from an external source. Please do not open attachments or click links unless this email comes from a known sender and you know the content is safe.



Ashishranjan - Domech Fabricators Pvt.Ltd.

unread,
6:40 AM (15 hours ago) 6:40 AM
to material...@googlegroups.com

If the operating temperature is high, I would seriously consider ERNiCr-3 (Alloy 82) rather than trying to solve the problem by moving from ER310 → ER309LMo.

Nickel-alloy fillers are frequently used for difficult dissimilar-metal joints because they tolerate the chemistry gradient/dilution between different alloys and can provide a more forgiving weld-metal structure. This is especially relevant if PWHT or substantial thermal cycling is involved.

Regards,

Ashish Ranjan

Go green logo

Save a tree...Please consider your environmental responsibility. Before printing this e-mail message, ask yourself whether you really need a hardcopy.



"Confidentiality Warning: This message and any attachments are intended only for the use of the intended recipient(s), are confidential and may be privileged. If you are not the intended recipient, you are hereby notified that any review, re-transmission, conversion to hard copy, copying, circulation or other use of this message and any attachments is strictly prohibited. If you are not the intended recipient, please notify the sender immediately by return email and delete this message and any attachments from your system.

Virus Warning: Although the company has taken reasonable precautions to ensure no viruses are present in this email. The company cannot accept responsibility for any loss or damage arising from the use of this email or attachment."


Caution: The e-mail below is from an external source. Please do not open attachments or click links unless this email comes from a known sender and you know the content is safe.


--

Kannayeram Gnanapandithan

unread,
10:31 AM (11 hours ago) 10:31 AM
to material...@googlegroups.com
316l 
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015, ISO 3834, EN 1090 & EN 15085, 
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Tue, Aug 11, 2026 at 3:46 PM hvala...@gmail.com <hvala...@gmail.com> wrote:
--
Reply all
Reply to author
Forward
0 new messages