Aluminum Bronze (C63000) to carbon steel welding.

395 views
Skip to first unread message

VMSS Siva

unread,
Mar 1, 2021, 10:21:49 PM3/1/21
to material...@googlegroups.com
Hi all,

Anybody having experience in Aluminum Bronze - C63000 to carbon steel welding (full penertration fillet weld) if so please share following details.
1. Type of filler wire - GTAW
2. Type of Electrode - SMAW.
3. Interpass temperature, Is it required to maintain interpass temp. With heating coil.
4. Heat input requirements if any. 
5. If no sound weld, what type of defects we can expect. 
6. Other than DP, what other NDT we can use to find defects if any. 


With regards, 
Siva

Kannayeram Gnanapandithan

unread,
Mar 2, 2021, 12:50:42 AM3/2/21
to materials-welding
ER CuAl-A2

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALN-m%3DDCubRRK0wvubPbmv_Xr%2BSWUEHHtjMrgdQTaEezy_1Y4w%40mail.gmail.com.

VMSS Siva

unread,
Mar 2, 2021, 10:15:05 PM3/2/21
to material...@googlegroups.com
C63000 contains Nickel, whereas ER CuAl-A2, does not contain Nickel, please re-confirm whether we can use or not. 

With regards
Siva

Rahul Rathod

unread,
Mar 2, 2021, 10:53:06 PM3/2/21
to material...@googlegroups.com
ERCuNiAl is best choice for your application but you can also weld with ERCuAl-A2, both are suitable for your application,

if your base metal thickness has above 8 mm go with gmaw welding process, 
you can weld directly as well as buttering in Carbon steel with same welding consumable as per given above,
preheat 250 C ° at AL Bronze base metal for up to 10-12 mm base thickness,






वसुधैव कुटुम्बकम्


 

Rahul J Rathod 

Senior Welding Technician 

What's up  +918155889118

Email:  welder....@gmail.com


 view my profile onLinkedInview my profile on facebookmy skype id



Kannayeram Gnanapandithan

unread,
Mar 3, 2021, 3:34:12 AM3/3/21
to materials-welding
ER CuAl-A2 is best for dissimilar, but u can also use CuNiAl

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

George Dilintas

unread,
Mar 3, 2021, 10:15:29 PM3/3/21
to material...@googlegroups.com
impossible from metallurgical point of view

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALN-m%3DDCubRRK0wvubPbmv_Xr%2BSWUEHHtjMrgdQTaEezy_1Y4w%40mail.gmail.com.


--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

avis...@gmail.com

unread,
Mar 3, 2021, 10:15:36 PM3/3/21
to material...@googlegroups.com
Thank you Mr. Pandithan and Mr. Rahul, got ER CuNiAl filler wire to weld.
I need details from those who really having practical experience on this welding, to know and understand the difficulties faced, if any.



On 3 Mar 2021, at 11:34 AM, Kannayeram Gnanapandithan <kgpan...@gmail.com> wrote:



pgos...@rogers.com

unread,
Mar 3, 2021, 11:10:03 PM3/3/21
to material...@googlegroups.com

Aluminum bronze C63000 is a Copper-Aluminum alloy. It’s not directly weldable to Carbon steel.  Use of a buffer layer on carbon steel either Cu-Ni (70/30 or 90/10) followed by welding with fillers of matching chemistry  to alloy C 63000 would be advisable.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

image003.png
Reply all
Reply to author
Forward
0 new messages