clad vessel

105 views
Skip to first unread message

Vanchinath S.A.

unread,
Jul 7, 2016, 11:17:19 PM7/7/16
to material...@googlegroups.com
Dear Experts,
 I am presenting a case for which I would like to have your valuable comments:

Case: clad equipment - Base material- CS (P1) 25mm thk,
clad material -- SS 316L , 3 mm thk
PWHT- required for the whole equipment ( base + clad)
clad provided for corrosion , not included in design calculation

Welding qualification carried out: 1) for base material with PWHT , 2) for restoration of cladding overlay procedure done on CS(P1) for 316L weld. with PWHT

 Is above qualified procedures OK for the equipment as per ASME Section IX para QW 217 (b).

with regards

vanchinath

pgoswami

unread,
Jul 7, 2016, 11:31:23 PM7/7/16
to material...@googlegroups.com

Hello Vanchinath,

 

The qualified procedures looks good and are in conformance with QW-217(b) , where the clad thickness is not included in the design and the clad is considered for corrosion  resistance only. In addition to QW-217(b) one has to meet all the applicable requirements of QW-453.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist ,

Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

 


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CA%2B6Tn1JzyXjgR3GRSNQiQ0EPFCCvA_vO21EEZHtFJSWGnyBd0g%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Nitin Shetty

unread,
Jul 11, 2016, 4:58:05 AM7/11/16
to material...@googlegroups.com
Dear sir,

You have specified the required wps based on the 2 portions which U need to weld and these 2 are only required. Since the requirement of clad is for corrosion purpose only U need to check the corrosion properties after simulating the coupons to the vessel pwht cycle. This requirement may not come code but from ur client spec.

Regards,

Nitin

Prakash Hegde

unread,
Jul 11, 2016, 9:15:54 AM7/11/16
to material...@googlegroups.com
Hi!
Yes
Provided the PQR meets the requirement of QW453 and with undiluted chemistry(316L) level from base of CRweld overlay and other requirement like IGC as per client spec
Regards
Hegde



For more options, visit https://groups.google.com/d/optout.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.