QW 451.1

18 views
Skip to first unread message

Rilley Chellah Mulenga

unread,
Feb 26, 2025, 8:41:44 AM2/26/25
to material...@googlegroups.com
Dear experts,

QW 451.1 takes about the qualification range limit and the tensile and bend tests requirement , working with a tests coupon of 38mm , is it okey to do root and face bend tests as opposed to side bend tests ?

--
Thanks & kind regards


EmailLogo      

www.ahkgroup.com     

    
     Rilley Chellah Mulenga
     HEAD - MATERIALS EVALUATION

     T: +260 212 226431
     M:+26076123880/ 0964084833
     E:Rilley.Mulenga@ahkgroup.com


DISCLAIMER: The information in this Internet e-mail is confidential and may be legally privileged. It is intended solely for the addressee(s).
Access to this Internet e-mail by anyone else is unauthorised.

If you are not the intended recipient, any disclosure, copying, distribution or any action taken or omitted to be taken in reliance on it, is prohibited and may be unlawful.
All results and data contained in this document are subject to our Standard Terms and Conditions and are valid only when supported by an original document.

Please visit our website at www.ahkgroup.com

Deerendra Karanth

unread,
Feb 26, 2025, 11:32:21 AM2/26/25
to material...@googlegroups.com

As per ASME Section IX, for test coupons greater than 10 mm (3/8 inch) in thickness, side bend tests are required. Since your test coupon is 38 mm thick, side bend tests should be conducted instead of root and face bend tests.

The reason for this requirement is that side bend tests effectively evaluate the entire thickness of the weld, ensuring that any discontinuities across the weld zone are detected.

BR, 

Deerendra 


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHkXHT8mZwBJeBtT3PGOta%3DLFe4CnBfzebXNCFYT8%2Bv9_0vwfQ%40mail.gmail.com.
Reply all
Reply to author
Forward
0 new messages