Greeting ALL,

On my project we are doing PWHT on Thickness basis, Pipe thickness is 30.18mm
,Will we do PWHT of Welded Supports as per B31.3? 


Bilal Arshad 
P.W.H.T QCI 

james gerald

unread,
Dec 16, 2020, 1:44:58 AM12/16/20
to material...@googlegroups.com
Generally the Pressure containing Pipe Thickness is taken as the Governing thickness when welding non-pressure part support.

But in the latest version of code there are some exceptions for some P-No's and if you could be specific it will be clear.

Thanks & Regards

J.Gerald Jayakumar




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMqL%2BROYYc4qzhMs9p%3Dr39KsXvUZXYe32G-CAYZ%2BBW3sj-K1wA%40mail.gmail.com.

bilal wahla

unread,
Dec 16, 2020, 2:08:10 AM12/16/20
to material...@googlegroups.com
Dear J.Gerald  ,
Material is P-1.



--
Respected Sir,

Please find the enclosed file.

Bilal Arshad Wahla

james gerald

unread,
Dec 16, 2020, 2:21:24 AM12/16/20
to material...@googlegroups.com
Preheat to 95degC prior to welding and use multilayers to avoid PWHT for P-1 material.

Only decrease in preheat temperature greater than 55degC is an essential variable as per ASME Sec.IX and hence revise the WPS to indicate preheat min 95degC without any need for qualifying PQR and perform welding.

Thanks & Regards

J.Gerald Jayakumar


bilal wahla

unread,
Dec 16, 2020, 2:45:46 AM12/16/20
to material...@googlegroups.com
Dear

can you please provide me with a reference.
And preheat is not mentioned in WPS.

james gerald

unread,
Dec 16, 2020, 3:13:28 AM12/16/20
to material...@googlegroups.com
Inline image



Just revise the WPS to include higher Preheat without qualifying the PQR.

Thanks & Regards

J.Gerald Jayakumar


George Dilintas

unread,
Dec 16, 2020, 10:47:11 PM12/16/20
to material...@googlegroups.com
Pwht is governed by the pressure part, not by the support. If the support is welded on a pressure part which must be pwhted then this weld will be pwhted

--