ROOT GAP QUALIFICATION WHEN QUALIFYING WPS/PQR/WPQ

496 views
Skip to first unread message

JAY

unread,
Jul 11, 2018, 6:50:12 AM7/11/18
to Materials & Welding
Dear Team,

I have some question in my mind regarding WPS/PQR/WPQ Qualifications. Explain below.

1. I have qualified wps with(SAME SEC IX)-
    Materials : SA 240 GR 316L TO SA 240 GR 316L (P8 G1 TO P8 G1)
    Process : GTAW.(with back gauge)
    Thickness: 8 mm to 8 mm.
    Root gap: 1.6 mm
 
     Now my question is about root gap qualification,
     If i qualify WPS with above parameters having root gap 1.6.The range qualification of thickness is 4 to 16 mm. likewise is there any range for Root gap qualification?

    YOUR ASSISTANCE IN THIS MATTER WOULD BE GREATLY APPRECIATED. 

Rajesh Kasvala

unread,
Jul 11, 2018, 8:16:06 AM7/11/18
to material...@googlegroups.com
Joint design non essentials veriable

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Nithin Joseph

unread,
Jul 11, 2018, 8:16:06 AM7/11/18
to material...@googlegroups.com
Dear,

There is no limit,  you can follow any root gap.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.



--
Regards,
Dsilva

syed moinul hasan

unread,
Jul 11, 2018, 10:18:56 PM7/11/18
to material...@googlegroups.com
Separately, There is no Root Gap qualification in code as its non-essential variable as per ASME IX.
Hence , cheers  go ahead and maintain the gap as appropriate. 

On Wed, 11 Jul 2018 at 16:16, Nithin Joseph <nithind...@gmail.com> wrote:
Dear,

There is no limit,  you can follow any root gap.
On Wed, Jul 11, 2018 at 9:04 AM, JAY <jay00...@gmail.com> wrote:
Dear Team,

I have some question in my mind regarding WPS/PQR/WPQ Qualifications. Explain below.

1. I have qualified wps with(SAME SEC IX)-
    Materials : SA 240 GR 316L TO SA 240 GR 316L (P8 G1 TO P8 G1)
    Process : GTAW.(with back gauge)
    Thickness: 8 mm to 8 mm.
    Root gap: 1.6 mm
 
     Now my question is about root gap qualification,
     If i qualify WPS with above parameters having root gap 1.6.The range qualification of thickness is 4 to 16 mm. likewise is there any range for Root gap qualification?

    YOUR ASSISTANCE IN THIS MATTER WOULD BE GREATLY APPRECIATED. 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.



--
Regards,
Dsilva

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

Prakash Gotimukul

unread,
Jul 11, 2018, 10:18:56 PM7/11/18
to materials-welding
Root gap is not an essential variable. It is based on skill of the welder. It is general practise to specify tolerznce as it is a fabrication work not machining. So you can say 1.5mm+1.5 mm

Rgds.
Prakash G  AIS

jay prajapati

unread,
Jul 11, 2018, 10:18:59 PM7/11/18
to material...@googlegroups.com
Dear,

As it is NON essential Variable. but is there any range/ limit up to which i can joint design? 

Ramesh

unread,
Jul 11, 2018, 10:19:00 PM7/11/18
to material...@googlegroups.com
Hi

QW-402.6  “ An increase in the fitup gap, beyond that initially qualified.”

 

For EBW,LBW it is Essential variable (QW 260 & QW 264)

For GTAW,  QW- 402.6 is not applicable / Not specified at all. 

 

Even for EBW,LBW, in case root gap is qualified with 1 mm, increase more than 1mm is not allowed. So there is No range of qualification.

 

For GTAW, it’s the ability of welder to fuse both roots to make smooth weld. I  have seen an welder done with 15mm gap without issues.

 

Better to strict with PQR root gap to achieve your production weld mechanical requirements / NDE requirements


Thanks and Regards


Rameshkannan Devaraj

"What you have learned is a mere handful; What you haven't learned is the size of the world – Avvaiyar"



jay prajapati

unread,
Jul 11, 2018, 10:19:00 PM7/11/18
to material...@googlegroups.com
Dear Joseph,

Is there any statement mentioned in standard?

On Wed, Jul 11, 2018 at 5:46 PM Nithin Joseph <nithind...@gmail.com> wrote:
Dear,

There is no limit,  you can follow any root gap.
On Wed, Jul 11, 2018 at 9:04 AM, JAY <jay00...@gmail.com> wrote:
Dear Team,

I have some question in my mind regarding WPS/PQR/WPQ Qualifications. Explain below.

1. I have qualified wps with(SAME SEC IX)-
    Materials : SA 240 GR 316L TO SA 240 GR 316L (P8 G1 TO P8 G1)
    Process : GTAW.(with back gauge)
    Thickness: 8 mm to 8 mm.
    Root gap: 1.6 mm
 
     Now my question is about root gap qualification,
     If i qualify WPS with above parameters having root gap 1.6.The range qualification of thickness is 4 to 16 mm. likewise is there any range for Root gap qualification?

    YOUR ASSISTANCE IN THIS MATTER WOULD BE GREATLY APPRECIATED. 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.



--
Regards,
Dsilva

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

Souravbohray

unread,
Jul 14, 2018, 2:00:33 AM7/14/18
to Materials & Welding
no root gap is come under joint design nd it is non essential variable nd sometime its depend upon welder.welding consumable dia.welding progression

Souravbohray

unread,
Jul 14, 2018, 2:00:33 AM7/14/18
to Materials & Welding
mr jay there is no statment regarding root gap. simple in wps u mention as per fabrication drawing in column of wps.i have experience of this nd i got guidline about this from ASME Authorised Inspector.dnt worry go ahead

jay prajapati

unread,
Jul 15, 2018, 10:13:33 PM7/15/18
to material...@googlegroups.com
Dear Sourav,

Thanks you so much for clear my doubt on this topic.

This is the only group from where i can get satisfactory answer.

Also humble request to Team, if there is any other groups related to engineering field like this,Then please share to explore  batter experience.    

On Sat, Jul 14, 2018 at 11:30 AM Souravbohray <ermechsou...@gmail.com> wrote:
mr jay there is no statment regarding root gap. simple in wps u mention as per fabrication drawing in column of wps.i have experience of this nd i got guidline about this from ASME Authorised Inspector.dnt worry go ahead

Er Sourav Bohray

unread,
Jul 15, 2018, 11:53:41 PM7/15/18
to material...@googlegroups.com
its ok and one more imp thing it is not compulsory to maintain uniform root gap throughout because in 3g position when moving upward more penetration required so need more gap but range should be not more than 2mm its mean at starting u make 2mm root gap but at upward 3 or 3.5 mm gap its ok.select consumable dia equal or less than root gap not more than root gap it vill cause lack of penetration.
This is best group i solve n learn about lot for my doubts its my daily routine to go through the posts of this group because all post n replies are based on experience sometime practical is more helpful than theory

You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/ROcnk05ckcQ/unsubscribe.