IGC-Test as per A262 Practice E

125 views
Skip to first unread message

Kannayeram Gnanapandithan

unread,
Mar 15, 2016, 1:49:42 AM3/15/16
to materials-welding
Experts comments on the following for any precautionary measured to be taken

Tube Matl--- ASS 316L

 Dimension--- Dia 38.1 X 4.06 mm thick

  R/D ratio=1

Cold bending followed by Solution Annealing ( Water or Air quencing, advice required to choose Air or Water),

Followed by IGC as per A262 Practice E

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY

PREM SHANKARDUTT NAUTIYAL

unread,
Mar 15, 2016, 11:31:37 PM3/15/16
to material...@googlegroups.com
I have mostly seen Tube manufacturers follow water quenching after Solution Annealing.

Only care you can take is ensure chloride content of water upto 25ppm max. and water quenching to be done immediately and should not exceed more than 3 minutes after SA.



PREM S NAUTIYAL
CELL : 9769316004
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eNYprQZ%2BXW2M%3DfAm0kyVLH85zNEo4zLWBR8LXpEqamCow%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Get your own FREE website, FREE domain & FREE mobile app with Company email.  
Know More >

BM

unread,
Mar 16, 2016, 2:44:02 AM3/16/16
to Materials & Welding
Are u referring to u-tubes? Solution annealing in the furnace may cause distortions, which affects tube insertion into bundle skeleton. You can use electrical resistance heating to heat the u bend portion plus some 50 to 75 mm on both straight lengths. On attaining the solution annealing temperature apply a blast of air to quench it. Usually possible in 2 minutes to bring to less than 375 degree C. Can purge with nitrogen or argon to prevent scaling inside. A mock up on a similar piece is helpful to establish the parameters - current, heating time, volume and time duration of air blast, tube thinning, ovality, etc. IGC test at electric contact zone may also be considered. Extra care required during bending of R= 38.1 to prevent OD collapse. Liquid penetrant test on the entire heated zone advisable.

George Dilintas

unread,
Mar 22, 2016, 11:24:58 AM3/22/16
to Meghanadh K
Why you don't follow the approach described in ASME BPVC Section VIII-1 / UHA-44?


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eNYprQZ%2BXW2M%3DfAm0kyVLH85zNEo4zLWBR8LXpEqamCow%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

Vishwas Keskar Welding Manager Pune India

unread,
Apr 17, 2016, 11:23:47 AM4/17/16
to Materials & Welding
Dear Sir,

Pl refer PG 19 of ASME SEC I OR UHA 44 of ASME SEC VIII DIV 1 before deciding Heat treatment . The strain and  service temperature , both shall be considered .

for 4.06 mm thk, Blat of air should suffice  and so the distortion etc 
Do a mock up test and plan accor 