Dear experts kindly guide me For GTAW 

1. Inconel 625 to SS 304H : what filler wire can be use 

2. Inconel 625 to SS316L : 
What filler wire can be use

Regards

Chandrasekaran V

Karthik

unread,
May 19, 2022, 11:16:53 PM5/19/22
to material...@googlegroups.com
Hi,
1. Inconel 625 to SS 304H : ENiCrFe-2 or ENiCrMo-3
2. Inconel 625 to SS316L : ENiCrFe-2 or ENiCrMo-3


Thanks& Regards,

(Karthik)
Karthikeyan.S
M: +66-892512282


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAN4ibzmvO7S7PhStVFoVfO%3D97tuRBY_f3_ak9Nz_hACR%3DEeTCw%40mail.gmail.com.

Kannayeram Gnanapandithan

unread,
May 23, 2022, 12:57:15 AM5/23/22
to materials-welding
625+304H it is better to NiCr3 or NiCr Fe2

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


james gerald

unread,
May 23, 2022, 2:43:35 AM5/23/22
to material...@googlegroups.com
Pandithan Sir,

For GTAW Welding - ERNiCr3

For SMAW Welding - ENiCrFe2

Thanks & Regards

J.Gerald Jayakumar



james gerald

unread,
May 23, 2022, 12:26:22 PM5/23/22
to material...@googlegroups.com
For dissimilar welding, RP582 recommends below.

Inline image


Thanks & Regards

J.Gerald Jayakumar


On Monday, 23 May, 2022, 09:02:41 am GMT+4, Kannayeram Gnanapandithan <kgpan...@gmail.com> wrote:


Reply all
Reply to author
Forward
0 new messages