Vacuum pack welding electrodes

2,373 views
Skip to first unread message

Jay Poojary

unread,
Sep 5, 2015, 2:14:13 AM9/5/15
to material...@googlegroups.com

Dear Experts,

Can anybody from our experts,  share some information regarding vacuum pack low hydrogen electrode. Specially about the baking of this electrodes,  if left out.

Thanks & regards,
Jay Poojary,
QA/QC ENGINEER
OCLLC,
NIGERIA

venkat chikkala

unread,
Sep 5, 2015, 3:06:20 AM9/5/15
to material...@googlegroups.com, jayo...@gmail.com
Dear Jay,

Vacuum packed Low hydrogen electrodes, may be used without baking, if, packing is not damaged.

If electrodes are exposed to atmosphere same to be baked as per electrode  manufacture requirements or as specified by client specification.

You may refer  Table 3 in SFA-5.1 in ASME Sec II part C for baking temperatures &  para 5.3 in  AWS D 1.1 ( addition 2004) for storage of Low hydrogen electrodes.

Regards,
CH V Ramana
Bureau Veritas (I) Pvt Ltd.





--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAAcO%3DyQMm2T39_y9OaL-17NAe5bZhwiOVXKoh2YKpqLWEKV4RQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


Jay Poojary

unread,
Sep 5, 2015, 1:07:02 PM9/5/15
to venkat chikkala, material...@googlegroups.com
Dear Mr.Venkat,

Thank you very much for your reply. It is of great useful to me.





cordially,
Jay Poojary

ashok rai

unread,
Sep 6, 2015, 12:09:06 AM9/6/15
to Materials & Welding
Dear Experts,

As a corollary to this, is there any need to vacuum pack any TIG Welding Rods?

Ashok Rai

deva m

unread,
Sep 6, 2015, 12:40:13 AM9/6/15
to material...@googlegroups.com

Tig rods are not needed to be vacuum packed since it does not contains flux/coatings which attracts moisture.

Regards

Dhevendran

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.

salman cader

unread,
Sep 6, 2015, 12:40:25 AM9/6/15
to material...@googlegroups.com

Bake 300-350'celcius
1-2 hours
Store 150'celcius shelf life
Small batches in heated quivers
70' celcius/quivers
Record no. of bakes / not more than 3
15ml/100g

Please not vacum packed electrodes dont get baked first time around because there is no water content.....so make sure this is true first......

--

RAJENDRA PRASAD TRIPATHI

unread,
Sep 10, 2015, 8:49:08 AM9/10/15
to Materials & Welding

Low hydrogen vacuum pack electrodes

 

It can be used without baking subject to intact packing . Keeping in view of practical problem of rebacking in project site where, every time controlling of rebacking is not possible, results hydrogen induced defects may be occur. To get rid of such problems we can use vacuum packed electrode. This vacuum pack will not only retain the minimum hydrogen level but also become ease to use the electrode without expensive rebacking at remote. It  can be put in portable oven maintaining temperature 70-80º C ready to use.  

But consumable should be properly vacuum packed as per process.  

 

 Advantage: 

·         No need of rebacking means we can save electricity and time. 

·          Reduction of Hydrogen induced crack.

·          To get minimum Hydrogen level in weld metal.


Thanks

Vinay Tripathi

India

9643886124


On Saturday, September 5, 2015 at 11:44:13 AM UTC+5:30, Jay Poojary wrote:

Alan Denney

unread,
Sep 10, 2015, 11:10:10 PM9/10/15
to material...@googlegroups.com

Anup N K E

unread,
Sep 11, 2015, 3:14:25 AM9/11/15
to material...@googlegroups.com
Dear Jay,


As per Aramco Standard requirement, vaccum packed electrodes (E7018) can be used for a maximum of four hours without using any baking or portable oven.  It can be used for eight hours if it continuously maintained at 60 degree in a portable oven. If the left over electrodes are to be used after eight hours , it needs to be re-dried.


Regards,

Anup


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
Reply all
Reply to author
Forward
0 new messages