Lethal service requirement

266 views
Skip to first unread message

sachin sankhe

unread,
Apr 2, 2016, 3:31:07 AM4/2/16
to material...@googlegroups.com
Dear Friends,

Need your opinion on below

Equipment
Columns

Design Code

ASME SEC VIII Div.1

Process 

High Wet H2S service(NACE)
Wet Amine service
Very Toxic
Lethal(ASME SEC VIII, UW-2)

Metallurgy/Thk
Base Metal MOC=SA516 Gr.70
Thk=8mm
Clad MOC=SS316L
Clad thk=3mm

Problem
Is PWHT mandatory for clad vessel for above process condition?
For lethal service is PWHT not mandatory for clad vessel as per Table UCS56.1 Note (e)

Regards
Sachin Sankhe






Get your own FREE website, FREE domain & FREE mobile app with Company email.  
Know More >

pgoswami

unread,
Apr 3, 2016, 12:11:47 AM4/3/16
to material...@googlegroups.com, sachin...@rediffmail.com, Mainak Mukherjee

Hi Sachin,

 

I hope API RECOMMENDED PRACTICE 945, Avoiding Environmental Cracking in Amine Units is refereed in the drawings. This is an essential document for amine service .As per this document use of austenitic S.S (304L/316L) clad steel is often done for amine plant equipments, for specific set of design conditions. That’s well taken care of in the details provided below.

 

As regarding fabrication, PWHT requirement is governed by the thickness of the backing material Carbon Steel, for regular amine service. From that aspect had this been a normal Amine vessel with 316L clad, exemption from PWHT would have been possible for 8 mm of C.S wall thickness.

 

Sec-VIII, UW-2 refers to mandatory PWHT for C.S/LAS vessels in “Lethal Service” . The same concept is applicable for clad vessels also, involving lethal service. Please see the latest ASME Code interpretations as below. Note there are two answers. My interpretation is to go with tracking No 9980 (since it’s latest and more detailed)

 

Hope this would help.

 

Thanks.

 

 


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/20160401172500.21291.qmail%40f5mail-224-128.rediffmail.com.
For more options, visit https://groups.google.com/d/optout.

Vijay Patre

unread,
Apr 3, 2016, 1:34:10 AM4/3/16
to material...@googlegroups.com

Dear Sachin,
Check your project specification & process data sheet requirements.

Technically you can perform perform PWHT.

Regards,
Vijay Patre

--

Kannayeram Gnanapandithan

unread,
Apr 3, 2016, 1:44:56 AM4/3/16
to materials-welding
why do want PWHT for 8mm thick??

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY

prem_nautiyal26

unread,
Apr 3, 2016, 3:07:40 AM4/3/16
to materials-welding
As per UW-2 PWHT shall be carried out.
Hope the same is carried out in WPS / PQR.
 
Regards 

Prem Nautiyal
9769316004



Sent from Samsung Mobile


-------- Original message --------
From: sachin sankhe
Date:01/04/2016 12:25 PM (GMT-05:00)
Subject: [MW:24612] Lethal service requirement

José Juan Jiménez Alejandro

unread,
Apr 3, 2016, 11:31:17 PM4/3/16
to material...@googlegroups.com

dili...@gmail.com

unread,
Apr 4, 2016, 12:41:33 AM4/4/16
to Kannayeram Gnanapandithan
Lethal service=high risk

Sent from my BlackBerry 10 smartphone.
From: Kannayeram Gnanapandithan
Sent: Κυριακή, 3 Απριλίου 2016 - 08:44
To: materials-welding
Subject: Re: [MW:24622] Lethal service requirement

dili...@gmail.com

unread,
Apr 4, 2016, 12:41:36 AM4/4/16
to pgoswami, sachin...@rediffmail.com, Mainak Mukherjee
The overlay us exempted but not the CS which is the stress bearing part.

Sent from my BlackBerry 10 smartphone.
From: pgoswami
Sent: Κυριακή, 3 Απριλίου 2016 - 07:11
Cc: sachin...@rediffmail.com; 'Mainak Mukherjee'
Subject: [MW:24618] RE: 24612] Lethal service requirement

Reply all