Thank you for your time to read my question.
 
I have to weld grade AISI 4130 with AISI 4140. Weld joint configuration is a groove weld 6inch dia.
 
Which electrode is suitable for welding these base metals together.
 
UTS of these parent metals is around 95 to110 ksi.
 
Thanks
 
Mhaskar Aly
FREE Christmas Animations for your email – by IncrediMail! Click Here!
xmas_girl_en.gif

Kathalingam Babu

unread,
Dec 14, 2010, 10:23:17 PM12/14/10
to material...@googlegroups.com
Hi
 
Use ER80SG (Root )/E10018-D2 (Filling& Capping) , with a minimum preheat of 150 deg cel. and
 
PWHT @650 deg. cel and soaking time depending on the hardness requirements  if any.
 
Thanks & Regards,
 
K. Babu
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
xmas_girl_en.gif

Elshan Feyzullayev

unread,
Dec 16, 2010, 5:22:52 AM12/16/10
to material...@googlegroups.com
Hi Aly,
 
Both of these steels are low alloy steels. E10018-D2 electrodes (e.g. OK 74.86 from ESAB) would be an ideal for these type of steels.
AISI 4130 is a good weldable in compare with AISI 4140. You need to follow a strict preaheating on 120-150 deg.C and apply PWHT straight after welding to relief the stress at 620 deg. with a soak time dependant on the thickness of to be welded parts. 
 
Due to the fact that these type of steels are prone to post weld cracking 100% RT is mandatory before and after PWHT.
 
If any question please feel free to contact.

Thanks,
Elshan.
Baku, Azerbaijan.

Date: Tue, 14 Dec 2010 21:48:58 +0300
From: mhask...@gmail.com
To: material...@googlegroups.com

Subject: [MW:8733] Welding electrode to weld AISI 4140 with AISI 4130

xmas_girl_en.gif
Reply all
Reply to author
Forward
0 new messages