Why ASME sec VIII div.1 is silent of heat treatment above lower transformation temp.I mean normalising is not mentioned any where.
As per ASME sec VIII div.1 if due to cold forming fibre elongation is more that 5% then it gives reference of UCS-56,where it mention only stress releiving.
In which code I can find Normalising requirment(Temp, Holding time,loading temp)
I am aware that temp of normalising is about 910 Deg.c & holding time is 1mm/min.But I need reference of code.

Regards
Sachin

pgoswami

unread,
Aug 16, 2010, 11:11:45 PM8/16/10
to material...@googlegroups.com

Hello Sachin,

See below the extract from ASME  Sec-VIII,DIV-1 on the requirements of post forming heat treatments. Yes the code mandates only stress relieving  as post forming heat treatment due to the fact that C.S /LAS can accommodate deformation strains, thus it's safe to perform post forming heat treatments  well below the lower critical (AC1) temperature.

Unless forming is done above upper critical temperature (AC3) re-normalizing is not required. Some of the rationale as per my thoughts  are as follows:-

  1. C.S and some LAS do not have appreciable changes in mechanical properties following forming below AC1 temperature under normal service environments.
  2. If the service media  is  such  so as to  cause environmental cracking such as SCC, then it would be dictated by process specific specifications such as NACE or appropriate API guidelines or specific requirements from process licensors.
  3. Normalizing causes changes of phases during heating and cooling. The resultant change of microstructure changes mechanical and other properties
  4. Normalizing is done in the mill under due care. Unless shops are well equipped, re-normalize  following forming may destroy material properties.
I hope this clarifies your query.
 
Thanks
 
Pradip Goswami,P.Eng.
Welding & Metallurgical Engineer/Specialist
Ontario Power Generation Inc.
Email-pgoswami@sympatico.ca,
  • UCS-79 FORMING SHELL SECTIONS AND HEADS- Vessel shell sections, heads, and other pressure boundary parts of carbon and low alloy steel plates fabricated by cold forming shall be heat treated subsequently(see UCS-56) when the resulting extreme fiber elongation is more than 5% from the as-rolled condition. For P-No.1 Group Nos. 1 and 2 materials the extreme fiber elongation may be as great as 40% when none of the following conditions exist:

(1)

The vessel will contain lethal substances either liquid or gaseous (see UW-2).

(2)

The material is not exempt from impact testing by the rules of this Division or impact testing is required by the material specification.

(3)

The thickness of the part before cold forming exceeds 58 in. (16 mm).

(4)

The reduction by cold forming from the as-rolled thickness is more than 10% at any location where the extreme fiber elongation exceeds 5%.

(5)

The temperature of the material during forming is in the range of 250°F to 900°F (120°C to 480°C).


From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of sachin sankhe
Sent: Monday, August 16, 2010 11:22 AM
To: material...@googlegroups.com
Subject: [MW:6522] Normalising requirment in code

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

sachin sankhe

unread,
Aug 17, 2010, 1:59:05 PM8/17/10
to material...@googlegroups.com
Dear Pradip,
Thanks for you reply
In that case does NACE MR0175/NACE MR0103/NACE RP0472 either of them specify normalising requirment?I mean holding time and holding period?

Regards
Sachin

On Tue, 17 Aug 2010 08:58:08 +0530 wrote

>
Hello Sachin,
See below the extract from ASME Sec-VIII,DIV-1 on the
requirements of post forming heat treatments. Yes the code mandates only stress
relieving as post forming heat treatment due to the fact that
C.S/LAS can accommodate deformation strains, thus it's safe to perform
post forming heat treatmentswell below the lower critical (AC1)
temperature.
Unless forming is done above upper critical temperature (AC3)
re-normalizing is not required. Some of the rationale as per my thoughts
are as follows:-



C.S and some LAS do not have appreciable changes in mechanical
properties following forming below AC1 temperature under normal service
environments.

If the servicemedia is such so as to
cause environmental cracking such as SCC, then it would be dictated by process
specific specifications such as NACE or appropriate API guidelines or specific
requirements from process licensors.

Normalizing causes changes of phases during heating and
cooling. The resultant change of microstructure changes mechanical and other
properties

Normalizing is done in the mill under due care. Unless shops are
well equipped, re-normalize following formingmay destroy material
properties.
I hope
this clarifies your query.

Thanks


Pradip Goswami,P.Eng.
Welding & Metallurgical
Engineer/Specialist

Ontario Power Generation Inc.
Email-p...@sympatico.ca,

pgos...@quickclic.net


UCS-79 FORMING SHELL SECTIONS
AND HEADS- Vessel shell sections, heads,
and other pressure boundary parts of carbon and low alloy steel plates
fabricated by cold forming shall be heat treated subsequently(see UCS-56) when
the resulting extreme fiber elongation is more
than 5% from the as-rolled condition. For
P-No.1 Group Nos. 1 and 2 materials the extreme fiber elongation may be as great as 40% when none of the
following conditions
exist:
(1) The vessel will contain lethal substances either liquid or
gaseous (see UW-2).
(2) The material is not exempt from impact testing by the rules of this Division or impact testing is required
by the material specification.
(3) The thickness of the part before cold forming exceeds 5⁄8 in. (16
mm).
(4) The
reduction by cold forming from the as-rolled
thickness is more than 10% at any location where the extreme fiber
elongation exceeds 5%.
(5) The
temperature of the material during forming
is in the range of 250°F to 900°F (120°C to 480°C).
>


From: material...@googlegroups.com
[mailto:material...@googlegroups.com] On Behalf Of sachin
sankhe
>Sent: Monday, August 16, 2010 11:22 AM
>To:
material...@googlegroups.com
>Subject: [MW:6522] Normalising
requirment in code
>
>
Hi,
>
>Why ASME sec VIII div.1 is silent of heat treatment above
lower transformation temp.I mean normalising is not mentioned any where.
>As
per ASME sec VIII div.1 if due to cold forming fibre elongation is more that 5%
then it gives reference of UCS-56,where it mention only stress releiving.
>In
which code I can find Normalising requirment(Temp, Holding time,loading
temp)
>I am aware that temp of normalising is about 910 Deg.c & holding
time is 1mm/min.But I need reference of code.
>
>Regards
>Sachin
>




--
>To post to this group, send email to
material...@googlegroups.com
>To unsubscribe from this group, send email
to materials-weld...@googlegroups.com
>For more options, visit
this group's bolg at http://materials-welding.blogspot.com/
>The
views expressed/exchnaged in this group are members personel views and meant for
educational purposes only, Users must take their own decisions w.r.t. applicable
code/standard/contract documents.
>



--
>
To post to this group, send email to material...@googlegroups.com
>
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
>
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>

Reply all
Reply to author
Forward
0 new messages