IMPACT TEST FAILLURE

瀏覽次數:125 次
跳到第一則未讀訊息

QA/QC

未讀,
2021年10月7日 凌晨4:23:352021/10/7
收件者:Materials & Welding
DEAR MASTER 

we have a test coupon 7.11 thichness with flange a106 with a105n 

during mechanical test the impact test for FLANGE FAILLURE IN HAZ  IN 3 POINT £

IS IT ACCEPTABLE 

J Prinsen

未讀,
2021年10月7日 清晨5:32:252021/10/7
收件者:materials-welding
No it is not,

Something went wrong with the thermal cycle during welding, heat-input/interpass to high will break down the impact thoughness

Regards


Jurgen Prinsen IWE
Metallurgist and welding engineer



Van: "QA/QC" <adnan...@gmail.com>
Aan: "materials-welding" <material...@googlegroups.com>
Verzonden: Donderdag 7 oktober 2021 10:16:23
Onderwerp: [MW:32549] IMPACT TEST FAILLURE

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b6717387-54eb-4c06-9748-9d4eddf4497dn%40googlegroups.com.

Prakash Hegde

未讀,
2021年10月7日 清晨7:34:162021/10/7
收件者:material...@googlegroups.com
Hi
In addition some time there is possiblity of improper.Heat treatment received to Forging and casting causing non uniformity of.req.grain structure for total cross section Causing failure in Impact test
Regards

Ahmed Rashed

未讀,
2021年10月7日 晚上11:14:442021/10/7
收件者:material...@googlegroups.com
Dears, 

I made PQR material A333 GR.6 (6" STD) welded by GTAW for Root pass (ER70S-6) and SMAW (E7018-1) for filling and cap according to ASME IX , B31.3.
Tensile test and bend test passed.
Impact test failed (for weld metal Av. 12 J) and for (HAZ Av. 8 J) at -55.6 degree celsius.

I don't know why the impact test failed !!!!! 

james gerald

未讀,
2021年10月7日 晚上11:44:452021/10/7
收件者:material...@googlegroups.com
A333 Gr.6 is permitted by ASME B31.3 to be used at minimum temperature of -46degC. See snap shot below.

Inline image

Moreover please look below for the limits of  welding consumable.

E7018 can be used only upto -45degC. See snapshot below.

Inline image



For lower temperatures please go for Nickel based steel consumables. see snap shot below.

Inline image


If your case is a subsize specimen with temperature reductions, then review your welding conditions carefully.





Thanks & Regards

J.Gerald Jayakumar



Perumal Govindan

未讀,
2021年10月8日 凌晨12:26:412021/10/8
收件者:material...@googlegroups.com
Hi

Please let me know the following:
1. Min and max UTS of the actual project material ( refer all the batches / heat numbers of MTCs) was manufactured and hope the same material was used to run the PQR/PQT.
2. What is the application of the material and the MDMT.

Above information is required for the welding consumables selection.

ER70S-6 is having high carbon compared to ER70S-2. So ER70S-6 is not preferrable for ASTM A333 Gr. 6 root runs.

Also, E7018-1 can be used until 70KSI of your project material UTS, if the actual UTS exceeds, we have to choose other electrode. 

Regards
Perumal Govindan 




james gerald

未讀,
2021年10月8日 凌晨1:39:412021/10/8
收件者:material...@googlegroups.com
Just to add if you are using a subsize specimen then below snapshot values are Applicable.

Inline image


Thanks & Regards

J.Gerald Jayakumar


Kannayeram Gnanapandithan

未讀,
2021年10月8日 凌晨2:45:132021/10/8
收件者:materials-welding
7018-1 is not for more than -45 deg celsius 

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


Ramon Briceno

未讀,
2021年10月9日 凌晨12:36:372021/10/9
收件者:material...@googlegroups.com
Dear Ahmed,

Please use E-8018-C1, it contains Ni 2.5% which is good to better thougness until -60C.

 E-7018-1 is limited -45C. It contains high Mn (1.6 %) only. Enough to get good thougnees until -45C.

Regards, 
Ramon Briceno
Metallurgical Engineer



Enviado desde mi smartphone Samsung Galaxy.


-------- Mensaje original --------
De: Ahmed Rashed <ara...@qituv.com>
Fecha: 2021/10/07 11:14 PM (GMT-04:00)
Asunto: Re: [MW:32552] IMPACT TEST FAILLURE

Mohd Siraj

未讀,
2022年2月9日 凌晨2:54:362022/2/9
收件者:Materials & Welding
check flange Mn %..if less than 1 ,there is strong chance of failure.. procure flange wit more than 1.05% Mn.

Vishwas Keskar

未讀,
2022年2月9日 凌晨3:37:272022/2/9
收件者:material...@googlegroups.com
THK 7.11 mm 
Following information is required 
At what temperature Impact was carried out?
What is the impact sample size when tested ?

Mohd Siraj

未讀,
2022年2月14日 凌晨12:15:092022/2/14
收件者:Materials & Welding
impact test shall be minimum design temp or mentioned in spec.
for size and 10x10x55 if not possible , you can use reduece size , in your case 5.5 is possible so need to consider reduce temperature...this all thing lab will take care!..