Dear Experts
                        Can 6G qualified welder can weld T,K,Y joints,yes or no.If yes why,if no why.
Why only 6GR qualified welder only can weld T K Y JOINTS?
What type of NDT required?
How to weekly Repair rate of welder.


Kannayeram Gnanapandithan

unread,
Jul 26, 2023, 4:25:13 AM7/26/23
to material...@googlegroups.com
As per AWS D1.1, 6GR is required

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAO8WSnGALirhW4vroU5hACX-VMQLLvxm4FrmX5dEfEMYb1v45g%40mail.gmail.com.

Vinoth kanna

unread,
Jul 26, 2023, 4:25:13 AM7/26/23
to material...@googlegroups.com
Hi Uma shankar,

1) 6G - welder - No 

2) 6GR welder -Yes, TKY -joints are partial penetration groove joints with limited access during welding.
                          R stands for restriction ring during performance qualification. 

3) TKY NDT   - Before welding - UT Lamination check.
                         After Welding- Wet magnetic particle testing & Angle probe-Ultrasonic testing. 

4) Repair Rate- Only applicable for Full penetration groove weld & butt weld only (Category A-CategoryA,B,C)
 


Regards 
Vinoth






sridhar cn

unread,
Jul 26, 2023, 11:00:04 PM7/26/23
to material...@googlegroups.com
      The answer is No. 
      Know the differences between their bevel preparations. Hope the following will help you understand them: 

·        The difference between the 6G and 6GR positions is the restriction ring and the bevel preparation. 6G is prepared 

     as a single 'vee' at 45 degrees position with the horizontal plane, while the 6GR bevel preparation is a single bevel 

     and the two connecting pipes have different thicknesses, one is thicker by at least 4-6mm.

·        What differentiates the 6G from the 6GR? 

·        Firstly, the difference between both is the R in the 6GR. The letter R indicates that 6GR welding consists of a restricting 

     ring. Another difference between the 6G and 6GR is the bevel preparation. Bevel preparation is a procedure done to 

     prepare the metal before one can start welding. The welder cuts a slope at a specific angle on the metal, particularly at 

     the edge.  

·        If you are familiar with the 6G and 6GR test positions, you will understand how important both are when welding pipe and 

     tubular structures.

·        Now let’s look at what the 6G and 6GR positions imply to help broaden our understanding of how they differ.

·        What’s the 6G all about?

·        Firstly, the 6G position is the type whereby your tubular weld joint has to be included at an angle of 45 degrees. It’s a difficult 

     test to pass, though not impossible. 

·        What is the 6GR all about? 

·        6GR turns out to be more challenging, you will find a restriction plate wrapped around the pipe’s circumference here. This plate 

     restricts the angle of the filler metal or electrode. And as a consequence of this restriction, welding becomes more challenging 

     than it should be.

·        So, when you find a 6GR welder, know that the said individual has successfully overcome the obstacle in this test piece and 

     welded it perfectly to have gotten that certification. The R means there’s an obstacle to overcome.

·        Further, another notable difference is that obtaining the 6G certificate qualifies a welder to weld pipe butt in all positions. On the 

     other hand, obtaining the 6GR certification means the welder is qualified to weld structural TKY connections.


C Sridhar.

 