I have following points to be clarified, please give your expert advise.

1) I have to do Procedure Qualification test as per ASME Sec. IX on a test coupon having 8 mm thk with Impact test at  -38 degree C, after machining the specimen size may be reduced to 10 x 5 x 55 or 10 x 6 x 55, in this case at what temperature I have to do 'V' notch  impact test and what will be the acceptable toughness value  as per ASME SEC VIII Div. I.

2) If we do procedure qualification test with impact test on P1 Gr. 2 to P1 Gr. 2  materials can I use this procedure qualification to weld P1 Gr 2 to P1 to Gr. 1 as per ASME Sec. IX.

Thanks in advance 

Manoj

RAJASEKARAN

unread,
Sep 23, 2012, 10:51:51 AM9/23/12
to material...@googlegroups.com

(1)       -49 C for (10x5), -46 C for (10x6) – Table UG 84.2

(2)       No

 

Raj

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

manoj john

unread,
Sep 25, 2012, 5:39:03 AM9/25/12
to material...@googlegroups.com
Dear Mr.Raj

Thanks for reply, and what will be the acceptable value at these temperature.

With Regards.
Mano

duc hoang

unread,
Sep 25, 2012, 11:25:44 PM9/25/12
to material...@googlegroups.com
Dear Mano

Please see UG-84(g)(5)

Regards
Dc

2012/9/25 manoj john <manoj...@gmail.com>

sevak hiren

unread,
Sep 26, 2012, 8:02:49 AM9/26/12
to material...@googlegroups.com
Also check SA 370 Table 9

duc hoang

unread,
Sep 26, 2012, 4:06:26 AM9/26/12
to material...@googlegroups.com

Sanjay Yadav

unread,
Sep 27, 2012, 6:46:02 AM9/27/12
to material...@googlegroups.com

Dear manoj
The values are proportional to the reduced area. Which means for 10x10 specimen required value is 20J than for 5x10 required value will be 10 J.
You can refer SA 370 for tabulated values