Cast iron to mild steel

148 views
Skip to first unread message

Pravin Poornachandran

unread,
Nov 2, 2020, 10:52:00 PM11/2/20
to 'Bijay' via Materials & Welding
Dear Expert, 

Good day.

I have to weld cast iron to mild steel.
What would be the suitable filler rod to use? 

Also is there any specific parameter or welding condition I have to follow since cast iron is difficult to weld. 

Example any specific heat treatment or post heating before welding? 

Kindly advice.

Best regards,
Pravin 

pgos...@rogers.com

unread,
Nov 2, 2020, 11:23:31 PM11/2/20
to material...@googlegroups.com

Hello Pravin

Cast iron is one of the difficult metals to weld. Grey cast irons are weldable subject to the original manufacturing process and grades involved. White cast irons are Unwedable. It’s important to know what’s the grade involved. Welding cast iron is typically a repair weld. Qualifying ASME Sec-IX procedures as like new fabrication  is quite difficult. One may have to settle with reduced angle of bending in “Guided Bend Test”. Some resources are attached for guidance.

Usually E-Ni-CI (99% Nickel) or ENiFe-CI(55%Ni) SMAW electrodes or GMAW fillers of equivalent composition are available for the consumable manufacturers.

If you want to know the subject well, get hold of this AWS publication.

Thanks.

 

P.Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

 

https://www.lincolnelectric.com/en-us/support/welding-how-to/Pages/welding-cast-iron-detail.aspx

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADDyn7eaVq1UvD%2BgBxN8BiwjvxLoa4MSduXQisFPpOo4fRfStA%40mail.gmail.com.


Virus-free. www.avg.com
fm99.pdf
Pages from AWS D11.2 - R2006 Guide for Welding Iron Castings.dat.pdf

Kannayeram Gnanapandithan

unread,
Nov 2, 2020, 11:43:33 PM11/2/20
to materials-welding
Use E NiFe-CI for cast iron to Steel
After welding it may be difficult for machining, if u want to go for machining after welding, Go with E Ni-Ci. 
Preheat, Interpass, slow cooling, peening of every burnt out electrode length  all are critical  to get good weldments. 

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


Pravin Poornachandran

unread,
Nov 5, 2020, 10:34:01 PM11/5/20
to material...@googlegroups.com
Dear Sir,

Thank you very much for your valuable advice on consumable selection. 

Appreciate it. 

Reply all
Reply to author
Forward
0 new messages